Specific Process Knowledge/Etch/DRIE-Pegasus/Isotropic: Difference between revisions
Appearance
No edit summary |
No edit summary |
||
| (17 intermediate revisions by the same user not shown) | |||
| Line 1: | Line 1: | ||
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/DRIE-Pegasus/Isotropic click here]''' | |||
<!--Checked for updates on 2/10-2020 - ok/jmli --> | |||
<!--Checked for updates on 14/5-2018 - ok/jmli --> | |||
<!--Checked for updates on 4/9-2025 - ok/jmli --> | |||
{| border="1" cellpadding="1" cellspacing="0" style="text-align:center;" | {| border="1" cellpadding="1" cellspacing="0" style="text-align:center;" | ||
| Line 7: | Line 10: | ||
! width="50"| Step | ! width="50"| Step | ||
! width="50"| Temperature | ! width="50"| Temperature | ||
! width="50"| Pressure | ! width="50"| Pressure | ||
! width="50"| C<sub>4</sub>F<sub>8</sub> | ! width="50"| C<sub>4</sub>F<sub>8</sub> | ||
| Line 18: | Line 20: | ||
! width="100" | Key words | ! width="100" | Key words | ||
|- | |- | ||
! | ! Mediumiso1 <!-- recipe name --> | ||
| - <!-- step --> | | - <!-- step --> | ||
| 20 <!-- chiller temp --> | | 20 <!-- chiller temp --> | ||
| 25 <!-- pressure --> | | 25 <!-- pressure --> | ||
| 0 <!-- C4F8 flow --> | | 0 <!-- C4F8 flow --> | ||
| Line 30: | Line 31: | ||
| 3 <!-- platen power --> | | 3 <!-- platen power --> | ||
|[[Specific Process Knowledge/Etch/DRIE-Pegasus/Isotropic/mediumiso1|1]] <!-- link processes --> | |[[Specific Process Knowledge/Etch/DRIE-Pegasus/Isotropic/mediumiso1|1]] <!-- link processes --> | ||
| | | Works great. Used extensively for Ph.D. thesis of Peter Emil Larsen <!-- keywords --> | ||
|- | |||
! Isoslow7 <!-- recipe name --> | |||
| - <!-- step --> | |||
| 10 <!-- chiller temp --> | |||
| 10 <!-- pressure --> | |||
| 0 <!-- C4F8 flow --> | |||
| 80 <!-- SF6 flow --> | |||
| 0 <!-- O2 flow --> | |||
| 0 <!-- Ar flow --> | |||
| 150 <!-- coil power --> | |||
| 3 <!-- platen power --> | |||
|[[Specific Process Knowledge/Etch/DRIE-Pegasus/Isotropic/Isoslow7|1]] <!-- link processes --> | |||
| <!-- keywords --> | |||
|- | |- | ||
! - <!-- recipe name --> | ! - <!-- recipe name --> | ||
| <!-- step --> | | <!-- step --> | ||
| <!-- chiller temp --> | | <!-- chiller temp --> | ||
| <!-- pressure --> | | <!-- pressure --> | ||
| <!-- C4F8 flow --> | | <!-- C4F8 flow --> | ||
| <!-- SF6 flow --> | | <!-- SF6 flow --> | ||
| <!-- O2 flow --> | | <!-- O2 flow --> | ||
| <!-- Ar flow --> | |||
| <!-- coil power --> | | <!-- coil power --> | ||
| <!-- platen power --> | | <!-- platen power --> | ||
| Line 45: | Line 59: | ||
| <!-- keywords --> | | <!-- keywords --> | ||
|- | |- | ||
|} | |} | ||
Latest revision as of 10:40, 4 September 2025
Feedback to this page: click here
| Recipe | Step | Temperature | Pressure | C4F8 | SF6 | O2 | Ar | Coil | Platen | Runs | Key words |
|---|---|---|---|---|---|---|---|---|---|---|---|
| Mediumiso1 | - | 20 | 25 | 0 | 150 | 0 | 0 | 600 | 3 | 1 | Works great. Used extensively for Ph.D. thesis of Peter Emil Larsen |
| Isoslow7 | - | 10 | 10 | 0 | 80 | 0 | 0 | 150 | 3 | 1 | |
| - |