Jump to content

Specific Process Knowledge/Thin film deposition/ALD Picosun R200/ALD multilayers: Difference between revisions

Eves (talk | contribs)
Eves (talk | contribs)
 
(53 intermediate revisions by 4 users not shown)
Line 1: Line 1:
This page describes non standart recipes including multilayers structures.
{{cc-nanolab}}


'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20https://labadviser.nanolab.dtu.dk//index.php?title=Specific_Process_Knowledge/Thin_film_deposition/ALD_Picosun_R200/ALD_multilayers click here]''' 
<br>
<br>
This page describes non-standart recipes including multilayers structures. They were the first test recipes on the ALD-1 to test the tool functionality and can be used as inspiration.
<br>
<br>
==Low temperature deposition of Al<sub>2</sub>O<sub>3</sub>==
==Low temperature deposition of Al<sub>2</sub>O<sub>3</sub>==


Line 29: Line 35:
Deposition rate: <b>0.089 nm/cycle </b>(@120 <sup>o</sup>C)
Deposition rate: <b>0.089 nm/cycle </b>(@120 <sup>o</sup>C)


This recipe has been developd for fabrication of high quality homogenious optical layers at low temperature.
This recipe has been developd for fabrication of high quality homogenious optical layers at low temperature. Research related results with this recipe can be found here: [http://journals.aps.org/prl/abstract/10.1103/PhysRevLett.115.177402 LINK - requires login] (Phys. Rev. Lett. 115(17) 2015, 177402)




Line 84: Line 90:
|}
|}


%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%
 
 
The uniformity, thickness, refractive index has been obtained using [[Specific_Process_Knowledge/Characterization/Optical_characterization#Ellipsometer|Ellipsometer VASE]].
 
 
<gallery caption="" widths="400px" heights="350px" perrow="2">
image:Al2O3_LT_Thickness.JPG| Measured thickness distribution across 100 mm wafer.
image:Al2O3_LT_RI.JPG| Measured refractive index distribution across 100 mm wafer.
</gallery>
 
<br clear="all" />
<b>Evgeniy Shkondin, DTU Nanolab, 2014-2016.</b>
<br clear="all" />
<br clear="all" />


==Low temperature deposition of TiO<sub>2</sub>==
==Low temperature deposition of TiO<sub>2</sub>==
Line 112: Line 131:
|}
|}


This recipe has been developd for fabrication of high quality homogenious optical layers at low temperature. The deposited TiO<sub>2</sub> layers are amorphous.
Deposition rate: <b>0.048 nm/cycle </b>(@ 120 <sup>o</sup>C)
 
This recipe has been developd for fabrication of high quality homogenious optical layers at low temperature. The deposited TiO<sub>2</sub> layers are amorphous. Research related results with this recipe can be found here: [http://journals.aps.org/prl/abstract/10.1103/PhysRevLett.115.177402 LINK - requires longin] (Phys. Rev. Lett. 115(17) 2015, 177402)




Line 124: Line 145:
| align="center" |  
| align="center" |  
{| border="2" cellspacing="2" cellpadding="3"  align="center" style="width:750px"
{| border="2" cellspacing="2" cellpadding="3"  align="center" style="width:750px"
! colspan="5" |Deposition conditions at 120 <sup>o</sup>C for Al2O3 LT recipe
! colspan="5" |Deposition conditions at 120 <sup>o</sup>C for TiO2 LT recipe
|-
|-
!Number of cycles
!Number of cycles
Line 168: Line 189:


%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%
%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%
Deposition rate: <b>0.048 nm/cycle </b>(@ 120 <sup>o</sup>C)
 
The uniformity, thickness, refractive index has been obtained using [[Specific_Process_Knowledge/Characterization/Optical_characterization#Ellipsometer|Ellipsometer VASE]].
 
 
<gallery caption="" widths="400px" heights="350px" perrow="2">
image:TiO2_LT_Thickness.JPG| Measured thickness distribution across 100 mm wafer.
image:TiO2_LT_RI.JPG| Measured refractive index distribution across 100 mm wafer.
</gallery>
 
<br clear="all" />
<b>Evgeniy Shkondin, DTU Nanolab, 2014-2016.</b>
<br clear="all" />
<br clear="all" />


==Low temperature grown multilayers on flat surfaces==
==Low temperature grown multilayers on flat surfaces==


Recipe: EMA01
<b>Recipe: EMA01</b>


Recipe: EMA02
<b>Recipe: EMA02</b>


Recipe: EMA03
<b>Recipe: EMA03</b>


Recipe: EMA04
<b>Recipe: EMA04</b>


Temperature: 120 <sup>o</sup>C
<b>Temperature: 120 <sup>o</sup>C</b>
 
All four recipes is based on <b>Al2O3_LT</b> amd <b>TiO2_LT</b> above mentioned low temperature recipes. Optical research based on fabricated Al<sub>2</sub>O<sub>3</sub> and TiO<sub>2</sub> multilayers has been published [http://journals.aps.org/prl/abstract/10.1103/PhysRevLett.115.177402 LINK] (Phys. Rev. Lett. 115(17) 2015, 177402)
 
 
<gallery caption="" widths="1000px" heights="700px" perrow="1">
image:multilayers222.jpg| Al<sub>2</sub>O<sub>3</sub>/TiO<sub>2</sub> multilayers.
</gallery>
 
<br clear="all" />
<b>Evgeniy Shkondin, DTU Nanolab (former DTU Danchip), 2014-2016.</b>
<br clear="all" />
<br clear="all" />
 
 
===Investigation of chemical composition in multilayers system===
 
Chemical tace analysis has been performed using [[Specific_Process_Knowledge/Characterization/XPS/K-Alpha|XPS K-Alpha]] equipment in depth profile mode.
 
<gallery caption="" widths="1000px" heights="1000px" perrow="1">
image:XPS_depth_multi_survey.JPG| Survey scan.
</gallery>
 
<br clear="all" />
 
<gallery caption="" widths="400px" heights="350px" perrow="2">
image:XPS_depth_Al_10_AL.jpg| Al 2p signal multilayers.
image:XPS_depth_Al_10_Ti.jpg| Ti 2p signal  multilayers.
image:XPS_depth_Al_10_O.jpg| O 1s signal  multilayers.
image:XPS_depth_Al_10_Si.jpg| Si 2p signal  multilayers.
</gallery>
 
<br clear="all" />
<b>Evgeniy Shkondin, DTU Nanolab (former DTU Danchip), 2014-2016.</b>
<br clear="all" />
<br clear="all" />


==Al<sub>2</sub>O<sub>3</sub>/TiO<sub>2</sub> multilayers on high aspect ratio structures==
==Al<sub>2</sub>O<sub>3</sub>/TiO<sub>2</sub> multilayers on high aspect ratio structures==
Line 189: Line 257:




<gallery caption="" widths="500px" heights="500px" perrow="2">
<gallery caption="" widths="1000px" heights="1000px" perrow="1">
image:Evgeniy Shkondin Si trenches coverd with Al2O3 and TiO2 multilayers using ALD.JPG| Al<sub>2</sub>O<sub>3</sub>/TiO<sub>2</sub> multilayers grown on silicon trenches.
image:Evgeniy Shkondin Si trenches coverd with Al2O3 and TiO2 multilayers using ALD.JPG| Al<sub>2</sub>O<sub>3</sub>/TiO<sub>2</sub> multilayers grown on silicon trenches.


Line 196: Line 264:


<br clear="all" />
<br clear="all" />
<b>Evgeniy Shkondin, DTU Danchip, 2014-2016.</b>