Jump to content

Specific Process Knowledge/Characterization/SEM Supra 1: Difference between revisions

From LabAdviser
Pevo (talk | contribs)
Pevo (talk | contribs)
 
(16 intermediate revisions by 3 users not shown)
Line 1: Line 1:
=<span style="background:#FF2800">THIS PAGE IS UNDER CONSTRUCTION</span>[[image:Under_construction.png|200px]]=
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Characterization/SEM_Supra_1  click here]'''
<!--Checked for updates on 30/7-2018 - ok/jmli -->


''This page is written by DTU Nanolab  internal''


'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Characterization/SEM_Supra_1  click here]'''
[[image:LA_SEM_Supra_1.jpg|400x400px|right|thumb|The SEM Supra 1 located in basement 346-907.{{photo1}} ]]
 
=SEM Supra 1=


[[image:LA_SEM_Supra_1.jpg|400x400px|right|thumb|The SEM Supra 1]]
The SEM Supra 1 is a scanning electron microscope (SEM). It produces enlarged images of a variety of specimens, achieving magnifications of over 500.000x providing ultra high resolution imaging. This important and widely used analytical tool provides exceptional resolution and depth of field, and minimal specimen preparation is required.


=SEM Supra 1=
This SEM is equipped two secondary electron (SE) detectors: An SE2 detector located on one side inside the chamber and an Inlens detector located inside the column. The SEM also has a backscatter electron detector: A BSD detector


The SEM Supra 1 a scanning electron microscope. It produces enlarged images of a variety of specimens, achieving magnifications of over 500.000x providing ultra high resolution imaging. This important and widely used analytical tool provides exceptional resolution and depth of field and requires minimal specimen preparation.
The SEM is a VP (variable pressure) instrument - Indicating that it is capable of operating at variable pressure. By increasing the pressure in the chamber and using a dedicated VPSE (Variable Pressure Secondary Electron) detector it is possible to image isolating samples. The higher density of gas molecules will eliminate the charges at the cost of slightly reduced resolution. Also, the SE2 and InLens detectors will no longer work.


The SEM is a VP (variable pressure) instrument - Indicating that it is capable of operating at variable pressure. By increasing the pressure in the chamber it is possible to image isolating samples. The higher density of gas molecules will eliminate the charges at the cost of slightly reduced resolution. Also, the HV detectors will no longer work.
The SEM is the training for fabrication SEM at DTU Nanolab. It means that all new SEM users with no or little SEM experience must be trained on this tool and gain basic knowledge here before being qualified for training on other SEM's.


The SEM is the training SEM at DTU Danchip. It means that all new SEM users with no and little SEM experience much be trained on this tool and gain basic knowledge (typically 10 hours of usage) here before being qualified for training on other SEM's.
The SEM Supra 1 was installed in the cleanroom in November 2010, but it has now been relocated in the basement outside the cleanroom, so that users can avoid to clean samples that have been outside the cleanroom before SEM inspection.  


The SEM Supra 1 (formerly known as SEM Zeiss) has been relocated to the basement with two purposes: Serving the users that have samples from outside the cleanroom and serving as training tool; all new SEM users with no/little SEM experience must be trained on this tool and gain basic knowledge (typically 10 hours of usage) here before being qualified for training on other SEM's.
The Sputter Coater 03 is located in the same room as the SEM Supra 1 and can be used to cover non-conductive samples (for instance glass or polymer samples) with a thin gold layer before SEM inspection to avoid charging problems.  


The SEM is located in basement outside the cleanroom. The Balzer Sputter is located in the same room and can be used to cover samples (for instance polymer samples from  the Polymer Injection Molding tool) with a thin gold layer before SEM inspection.  
Only users with samples that are somehow related to the work taking place in building 346 and 347 (the characterization part of DTU Nanolab). Other users will have to use the SEMs in building 314 (the characterization part of DTU Nanolab).  


The SEM LEO was installed in the cleanroom in the 1998, and the software was ungraded in 2012.




'''The user manual, control instruction, the user APV and contact information can be found in LabManager:'''
'''The user manual, control instruction, the user APV and contact information can be found in LabManager:'''


[http://labmanager.dtu.dk/function.php?module=Machine&view=view&page_id=169 SEM Supra 1 info page in LabManager],
[http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=275 SEM Supra 1 info page in LabManager],




Line 30: Line 33:
*[[Specific Process Knowledge/Characterization/SEM: Scanning Electron Microscopy|SEM comparison page]]
*[[Specific Process Knowledge/Characterization/SEM: Scanning Electron Microscopy|SEM comparison page]]


==Equipment performance and process related parameters==
 
==Equipment performance==


{| border="2" cellspacing="0" cellpadding="2"  
{| border="2" cellspacing="0" cellpadding="2"  
Line 40: Line 44:
|style="background:LightGrey; color:black"|Imaging and measurement of
|style="background:LightGrey; color:black"|Imaging and measurement of
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Any sample except bulk insulators such as polymers, glass or quartz wafers
* Conducting samples
* Semi-conducting samples
* Thin (~ 5 µm <) layers of non-conducting materials such as polymers
* Thick polymers, glass or quartz samples
|-
|-
!style="background:silver; color:black;" align="center" width="60"|Location  
!style="background:silver; color:black;" align="center" width="60"|Location  
|style="background:LightGrey; color:black"|
|style="background:LightGrey; color:black"|
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Basement of DTU Danchip
*Basement of building 346
|-
|-
!style="background:silver; color:black;" align="center" width="60"|Performance
!style="background:silver; color:black;" align="center" width="60"|Performance
Line 90: Line 97:
*Any standard cleanroom material and samples from the Laser Micromachining tool and the Polymer Injection Molding tool
*Any standard cleanroom material and samples from the Laser Micromachining tool and the Polymer Injection Molding tool
|-  
|-  
|}
===Quality control of length measurement ===
{| border="1" cellspacing="2" cellpadding="2" colspan="3"
|bgcolor="#98FB98" |'''Quality Control (QC) for SEM Supra 1'''
|-
|
*[http://labmanager.dtu.dk/d4Show.php?id=2493&mach=275 QC procedure for SEM Supra 1]<br>
*[https://labmanager.dtu.dk/view_binary.php?type=data&mach=275 Newest QC data for SEM Supra 1]<br>
'''QC limits:'''
{| {{table}}
| align="center" valign="top"|
{| border="2" cellspacing="1" cellpadding="2" align="center" style="width:500px"
! Detector
! Settings
! Magnification
! Measured dimensions
! Calibration limit
! Action limit
|-
|SE2
| EHT 10 kV, WD 10 mm
| 2.500 k
| 70x70 μm
| ± 2 %
| ± 3 %
|-
|SE2
| EHT 10 kV, WD 10 mm
| 17.000 k
| 10x10 μm
| ± 2 %
| ± 3 %
|-
|SE2
| EHT 5 kV, WD 5 mm
| 17.000 k
| 10x10 μm
| ± 2 %
| ± 3 %
|-
| VPSE
| EHT 10 kV, WD 10 mm, 17 Pa
| 17.000 k
| 10x10 μm
| ± 2 %
| ± 3 %
|-
| InLens
| EHT 5 kV, WD 5 mm
| 200.000 k
| 1x1 μm
| ± 2 %
| ± 3 %
|-
| InLens
| EHT 10 kV, WD 3 mm
| 1.000.000 k
| (imaging only)
| NA
| NA
|-
|}
|-
|}
|}
|}

Latest revision as of 15:54, 4 August 2025

Feedback to this page: click here

This page is written by DTU Nanolab internal

The SEM Supra 1 located in basement 346-907.Photo: DTU Nanolab internal

SEM Supra 1

The SEM Supra 1 is a scanning electron microscope (SEM). It produces enlarged images of a variety of specimens, achieving magnifications of over 500.000x providing ultra high resolution imaging. This important and widely used analytical tool provides exceptional resolution and depth of field, and minimal specimen preparation is required.

This SEM is equipped two secondary electron (SE) detectors: An SE2 detector located on one side inside the chamber and an Inlens detector located inside the column. The SEM also has a backscatter electron detector: A BSD detector

The SEM is a VP (variable pressure) instrument - Indicating that it is capable of operating at variable pressure. By increasing the pressure in the chamber and using a dedicated VPSE (Variable Pressure Secondary Electron) detector it is possible to image isolating samples. The higher density of gas molecules will eliminate the charges at the cost of slightly reduced resolution. Also, the SE2 and InLens detectors will no longer work.

The SEM is the training for fabrication SEM at DTU Nanolab. It means that all new SEM users with no or little SEM experience must be trained on this tool and gain basic knowledge here before being qualified for training on other SEM's.

The SEM Supra 1 was installed in the cleanroom in November 2010, but it has now been relocated in the basement outside the cleanroom, so that users can avoid to clean samples that have been outside the cleanroom before SEM inspection.

The Sputter Coater 03 is located in the same room as the SEM Supra 1 and can be used to cover non-conductive samples (for instance glass or polymer samples) with a thin gold layer before SEM inspection to avoid charging problems.

Only users with samples that are somehow related to the work taking place in building 346 and 347 (the characterization part of DTU Nanolab). Other users will have to use the SEMs in building 314 (the characterization part of DTU Nanolab).


The user manual, control instruction, the user APV and contact information can be found in LabManager:

SEM Supra 1 info page in LabManager,


Performance information


Equipment performance

Equipment SEM Supra 1 (Supra 40VP SEM)
Purpose Imaging and measurement of
  • Conducting samples
  • Semi-conducting samples
  • Thin (~ 5 µm <) layers of non-conducting materials such as polymers
  • Thick polymers, glass or quartz samples
Location
  • Basement of building 346
Performance Resolution
  • 1-2 nm (limited by vibrations)

The resolution is strongly dependent on the type of sample and the skills of the operator.

Instrument specifics Detectors
  • Secondary electron (Se2)
  • Inlens secondary electron (Inlens)
  • 4 Quadrant Backscatter electron (QBSD)
  • Variable pressure secondary electron (VPSE)
Stage
  • X, Y: 130 × 130 mm
  • T: -4 to 70o
  • R: 360o
  • Z: 50 mm
Electron source
  • FEG (Field Emission Gun) source
Operating pressures
  • Fixed at High vacuum (2 × 10-4mbar - 10-6mbar)
  • Variable at Low vacuum (0.1 mbar - 2 mbar)
Options
  • All software options available
Substrates Batch size
  • Up to 6" wafer with full view
Allowed materials
  • Any standard cleanroom material and samples from the Laser Micromachining tool and the Polymer Injection Molding tool

Quality control of length measurement

Quality Control (QC) for SEM Supra 1

QC limits:

Detector Settings Magnification Measured dimensions Calibration limit Action limit
SE2 EHT 10 kV, WD 10 mm 2.500 k 70x70 μm ± 2 % ± 3 %
SE2 EHT 10 kV, WD 10 mm 17.000 k 10x10 μm ± 2 % ± 3 %
SE2 EHT 5 kV, WD 5 mm 17.000 k 10x10 μm ± 2 % ± 3 %
VPSE EHT 10 kV, WD 10 mm, 17 Pa 17.000 k 10x10 μm ± 2 % ± 3 %
InLens EHT 5 kV, WD 5 mm 200.000 k 1x1 μm ± 2 % ± 3 %
InLens EHT 10 kV, WD 3 mm 1.000.000 k (imaging only) NA NA