Specific Process Knowledge/Etch/ICP Metal Etcher/silicon oxide/By Peixiong: Difference between revisions

From LabAdviser
Bghe (talk | contribs)
Bghe (talk | contribs)
No edit summary
 
(27 intermediate revisions by the same user not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/ICP_Metal_Etcher/silicon_oxide/By_Peixiong click here]'''
<br> {{CC-bghe1}} <br>
=With C4F8 and H2 chemistry (all tests done by Peixiong Shi, DTU Nanolab)=
==Part 1==
{|  class=MsoNormalTable border=0 cellspacing=0 cellpadding=0 width=855 style='width:641.0pt;border-collapse:collapse'  style='height:36.0pt'
|  width=83 valign=top style='width:62.0pt;border:solid white 1.0pt;  border-bottom:solid white 3.0pt;background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;  height:36.0pt' |
|  width=68 valign=top style='width:51.0pt;border-top:solid white 1.0pt;  border-left:none;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;  background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:36.0pt' |
|  width=81 valign=top style='width:61.0pt;border-top:solid white 1.0pt;  border-left:none;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;  background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:36.0pt' | <p class=MsoNormal><span lang=DA>Very good</span></p>
|  width=72 valign=top style='width:54.0pt;border-top:solid white 1.0pt;  border-left:none;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;  background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:36.0pt' | <p class=MsoNormal><span lang=DA>Very good</span></p>
|  width=79 valign=top style='width:59.0pt;border-top:solid white 1.0pt;  border-left:none;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;  background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:36.0pt' | <p class=MsoNormal><span lang=DA>Very good</span></p>
|  width=79 valign=top style='width:59.0pt;border-top:solid white 1.0pt;  border-left:none;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;  background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:36.0pt' | <p class=MsoNormal><span lang=DA>Very good</span></p>
|  width=79 valign=top style='width:59.0pt;border-top:solid white 1.0pt;  border-left:none;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;  background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:36.0pt' | <p class=MsoNormal><span lang=DA>Very good</span></p>
|  width=79 valign=top style='width:59.0pt;border-top:solid white 1.0pt;  border-left:none;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;  background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:36.0pt' | <p class=MsoNormal><span lang=DA>Very good</span></p>
|  width=79 valign=top style='width:59.0pt;border-top:solid white 1.0pt;  border-left:none;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;  background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:36.0pt' | <p class=MsoNormal><span lang=DA>Unstable plasma at 2mtorr</span></p>
|  width=79 valign=top style='width:59.0pt;border-top:solid white 1.0pt;  border-left:none;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;  background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:36.0pt' | <p class=MsoNormal><span lang=DA>stable plasma at 2.5mtorr</span></p>
|  width=79 valign=top style='width:59.0pt;border-top:solid white 1.0pt;  border-left:none;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;  background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:36.0pt' | <p class=MsoNormal><span lang=DA>stable plasma at 2.5mtorr</span></p>
|-  style='height:36.0pt'
|  width=83 valign=top style='width:62.0pt;border-top:none;border-left:solid white 1.0pt;  border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;background:  #4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:36.0pt' | <p class=MsoNormal>ICP metal etch SiO2 by reist mask try</p>
|  width=68 valign=top style='width:51.0pt;border-top:none;border-left:none;  border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;background:  #4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:36.0pt' | <p class=MsoNormal><span lang=DA>Date</span></p>
|  width=81 valign=top style='width:61.0pt;border-top:none;border-left:none;  border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;background:  #4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:36.0pt' | <p class=MsoNormal><span lang=DA>Feb262013</span></p>
|  width=72 valign=top style='width:54.0pt;border-top:none;border-left:none;  border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;background:  #4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:36.0pt' | <p class=MsoNormal><span lang=DA>Feb272013</span></p>
|  width=79 valign=top style='width:59.0pt;border-top:none;border-left:none;  border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;background:  #4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:36.0pt' | <p class=MsoNormal><span lang=DA>Feb272013 20:00</span></p>
|  width=79 valign=top style='width:59.0pt;border-top:none;border-left:none;  border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;background:  #4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:36.0pt' | <p class=MsoNormal><span lang=DA>Feb272013 23:00</span></p>
|  width=79 valign=top style='width:59.0pt;border-top:none;border-left:none;  border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;background:  #4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:36.0pt' | <p class=MsoNormal><span lang=DA>Feb282013 1am</span></p>
|  width=79 valign=top style='width:59.0pt;border-top:none;border-left:none;  border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;background:  #4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:36.0pt' | <p class=MsoNormal><span lang=DA>Feb282013 2am</span></p>
|  width=79 valign=top style='width:59.0pt;border-top:none;border-left:none;  border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;background:  #4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:36.0pt' | <p class=MsoNormal><span lang=DA>Feb282013 2am</span></p>
|  width=79 valign=top style='width:59.0pt;border-top:none;border-left:none;  border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;background:  #4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:36.0pt' | <p class=MsoNormal><span lang=DA>Feb282013 2am</span></p>
|  width=79 valign=top style='width:59.0pt;border-top:none;border-left:none;  border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;background:  #4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:36.0pt' | <p class=MsoNormal><span lang=DA>Feb2820134am</span></p>
|-  style='height:30.15pt'
|  width=83 valign=top style='width:62.0pt;border-top:none;border-left:solid white 1.0pt;  border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;background:  #4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:30.15pt' |
|  width=68 valign=top style='width:51.0pt;border-top:none;border-left:none;  border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;background:  #4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:30.15pt' | <p class=MsoNormal><span lang=DA>Metal ICP  recipe</span></p>
|  width=81 valign=top style='width:61.0pt;border-top:none;border-left:none;  border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;background:  #4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:30.15pt' | <p class=MsoNormal><span lang=DA>pxSiO2try5</span></p>
|  width=72 valign=top style='width:54.0pt;border-top:none;border-left:none;  border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;background:  #4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:30.15pt' | <p class=MsoNormal><span lang=DA>pxSiO2try6</span></p>
|  width=79 valign=top style='width:59.0pt;border-top:none;border-left:none;  border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;background:  #4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:30.15pt' | <p class=MsoNormal><span lang=DA>pxSiO2try7</span></p>
|  width=79 valign=top style='width:59.0pt;border-top:none;border-left:none;  border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;background:  #4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:30.15pt' | <p class=MsoNormal><span lang=DA>pxSiO2try8</span></p>
|  width=79 valign=top style='width:59.0pt;border-top:none;border-left:none;  border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;background:  #4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:30.15pt' | <p class=MsoNormal><span lang=DA>pxSiO2try8</span></p>
|  width=79 valign=top style='width:59.0pt;border-top:none;border-left:none;  border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;background:  #4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:30.15pt' | <p class=MsoNormal><span lang=DA>pxSiO2try8</span></p>
|  width=79 valign=top style='width:59.0pt;border-top:none;border-left:none;  border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;background:  #4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:30.15pt' | <p class=MsoNormal><span lang=DA>pxSiO2try9</span></p>
|  width=79 valign=top style='width:59.0pt;border-top:none;border-left:none;  border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;background:  #4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:30.15pt' | <p class=MsoNormal><span lang=DA>pxSiO2try9</span></p>
|  width=79 valign=top style='width:59.0pt;border-top:none;border-left:none;  border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;background:  #4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:30.15pt' | <p class=MsoNormal><span lang=DA>pxSiO2try9</span></p>
|-  style='height:33.3pt'
|  width=83 style='width:62.0pt;border-top:none;border-left:solid white 1.0pt;  border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;background:  #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:33.3pt' |
|  width=68 style='width:51.0pt;border-top:none;border-left:none;border-bottom:  solid white 3.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:33.3pt' | <p class=MsoNormal><span lang=DA>Wafer size and ID</span></p>
|  width=81 style='width:61.0pt;border-top:none;border-left:none;border-bottom:  solid white 3.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:33.3pt' | <p class=MsoNormal><span lang=DA>6inch,</span></p><p class=MsoNormal><span lang=DA>6A1_feb252013</span></p>
|  width=72 style='width:54.0pt;border-top:none;border-left:none;border-bottom:  solid white 3.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:33.3pt' | <p class=MsoNormal><span lang=DA>6inch,</span></p><p class=MsoNormal><span lang=DA>6A4_feb262013</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 3.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:33.3pt' | <p class=MsoNormal><span lang=DA>6inch,</span></p><p class=MsoNormal><span lang=DA>6A6_feb262013</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 3.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:33.3pt' | <p class=MsoNormal><span lang=DA>6inch,</span></p><p class=MsoNormal><span lang=DA>6A2_feb272013</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 3.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:33.3pt' | <p class=MsoNormal><span lang=DA>6inch,</span></p><p class=MsoNormal><span lang=DA>6A3_feb272013</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 3.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:33.3pt' | <p class=MsoNormal><span lang=DA>6inch,</span></p><p class=MsoNormal><span lang=DA>6A4_feb272013</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 3.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:33.3pt' | <p class=MsoNormal><span lang=DA>6inch,</span></p><p class=MsoNormal><span lang=DA>6A5_feb272013</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 3.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:33.3pt' | <p class=MsoNormal><span lang=DA>6inch,</span></p><p class=MsoNormal><span lang=DA>6A5_feb272013</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 3.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:33.3pt' | <p class=MsoNormal><span lang=DA>6inch,</span></p><p class=MsoNormal><span lang=DA>6A6_feb272013</span></p>
|-  style='height:71.7pt'
|  width=83 style='width:62.0pt;border:solid white 1.0pt;border-top:none;  background:#D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:71.7pt' |
|  width=68 style='width:51.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:71.7pt' | <p class=MsoNormal><span lang=DA>Mask</span></p>
|  width=81 style='width:61.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:71.7pt' | <p class=MsoNormal>440nm resist on 62nmBarc on 1800nm apox, first etch barc
20sec by Ox plasma</p>
|  width=72 style='width:54.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:71.7pt' | <p class=MsoNormal>440nm resist on 62nmBarc on 1800nm apox, first etch barc
20sec by Ox plasma</p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:71.7pt' | <p class=MsoNormal>780nm resist on 62nmBarc on 1800nm apox, first etch barc
20sec by Ox plasma</p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:71.7pt' | <p class=MsoNormal>780nm resist on 62nmBarc on 800nm apox, first etch barc
20sec by Ox plasma</p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:71.7pt' | <p class=MsoNormal>780nm resist on 62nmBarc on 490nm apox, first etch barc
20sec by Ox plasma</p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:71.7pt' | <p class=MsoNormal><span lang=DA>Blank Si</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:71.7pt' | <p class=MsoNormal>780nm resist on 62nmBarc on 490nm apox, first etch barc
20sec by Ox plasma</p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:71.7pt' | <p class=MsoNormal>780nm resist on 62nmBarc on 490nm apox, first etch barc
20sec by Ox plasma</p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:71.7pt' | <p class=MsoNormal>780nm resist on 62nmBarc on 490nm apox, first etch barc
20sec by Ox plasma</p>
|-  style='height:29.25pt'
|  width=83 style='width:62.0pt;border:solid white 1.0pt;border-top:none;  background:#E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' |
|  width=68 style='width:51.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>Etch time</span></p>
|  width=81 style='width:61.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>2min</span></p>
|  width=72 style='width:54.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>4min</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>4min</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>4min</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>5min</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>4min</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>1min</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>4min</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>5min</span></p>
|-  style='height:29.25pt'
|  width=83 style='width:62.0pt;border:solid white 1.0pt;border-top:none;  background:#E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' |
|  width=68 style='width:51.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>Pressure [mTorr] </span></p>
|  width=81 style='width:61.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>6</span></p>
|  width=72 style='width:54.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>6</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>4</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>3</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>3</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>2</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>2</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>2.5</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>2.5</span></p>
|-  style='height:29.25pt'
|  width=83 style='width:62.0pt;border:solid white 1.0pt;border-top:none;  background:#E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' |
|  width=68 style='width:51.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>C4F8 flow [sccm] </span></p>
|  width=81 style='width:61.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>0</span></p>
|  width=72 style='width:54.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>20</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>10</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>8</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>8</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>8</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>8</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>8</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>8</span></p>
|-  style='height:29.25pt'
|  width=83 style='width:62.0pt;border:solid white 1.0pt;border-top:none;  background:#E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' |
|  width=68 style='width:51.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>CF4 flow [sccm] </span></p>
|  width=81 style='width:61.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>40</span></p>
|  width=72 style='width:54.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>0</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>0</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>0</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>0</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>0</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>0</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>0</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>0</span></p>
|-  style='height:29.25pt'
|  width=83 style='width:62.0pt;border:solid white 1.0pt;border-top:none;  background:#E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' |
|  width=68 style='width:51.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>H2 flow [sccm] </span></p>
|  width=81 style='width:61.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>30</span></p>
|  width=72 style='width:54.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>20</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>30</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>30</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>30</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>30</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>30</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>30</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>30</span></p>
|-  style='height:29.25pt'
|  width=83 style='width:62.0pt;border:solid white 1.0pt;border-top:none;  background:#E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' |
|  width=68 style='width:51.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>CH4 flow [sccm] </span></p>
|  width=81 style='width:61.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>0</span></p>
|  width=72 style='width:54.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>Set 20 real 3.7</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>Set 20 real 3.7</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>0</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>0</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>0</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>0</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>0</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>0</span></p>
|-  style='height:29.25pt'
|  width=83 style='width:62.0pt;border:solid white 1.0pt;border-top:none;  background:#E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' |
|  width=68 style='width:51.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>Coil Power [W] </span></p>
|  width=81 style='width:61.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>800</span></p>
|  width=72 style='width:54.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>800</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>800</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>800</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>800</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>800</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>800</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>800 reflect 13W</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>800 reflect 8W</span></p>
|-  style='height:29.25pt'
|  width=83 style='width:62.0pt;border:solid white 1.0pt;border-top:none;  background:#D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' |
|  width=68 style='width:51.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>Platen Power [W] </span></p>
|  width=81 style='width:61.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>100</span></p>
|  width=72 style='width:54.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>100</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>120</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>150</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>150</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>150</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>150</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>150</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>150reflect 0.2w</span></p>
|-  style='height:33.3pt'
|  width=83 style='width:62.0pt;border:solid white 1.0pt;border-top:none;  background:#E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:33.3pt' |
|  width=68 style='width:51.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:33.3pt' | <p class=MsoNormal><span lang=DA>Platen temperature [<sup>o</sup>C] </span></p>
|  width=81 style='width:61.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:33.3pt' | <p class=MsoNormal><span lang=DA>20</span></p>
|  width=72 style='width:54.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:33.3pt' | <p class=MsoNormal><span lang=DA>20</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:33.3pt' | <p class=MsoNormal><span lang=DA>20</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:33.3pt' | <p class=MsoNormal><span lang=DA>20</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:33.3pt' | <p class=MsoNormal><span lang=DA>20</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:33.3pt' | <p class=MsoNormal><span lang=DA>20</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:33.3pt' | <p class=MsoNormal><span lang=DA>20</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:33.3pt' | <p class=MsoNormal><span lang=DA>20</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:33.3pt' | <p class=MsoNormal><span lang=DA>20</span></p>
|-  style='height:29.25pt'
|  width=83 style='width:62.0pt;border:solid white 1.0pt;border-top:none;  background:#D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' |
|  width=68 style='width:51.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>Coil match</span></p>
|  width=81 style='width:61.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>60%,27%</span></p>
|  width=72 style='width:54.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>63%,25%</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>63%,25%</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>67%,24%</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>67%,24%</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>68.9%,24.1%</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>68.9%,24.1%</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>68.7%,25.3%</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>68.87%,23.1%</span></p>
|-  style='height:29.25pt'
|  width=83 style='width:62.0pt;border:solid white 1.0pt;border-top:none;  background:#D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' |
|  width=68 style='width:51.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>Platen Match</span></p>
|  width=81 style='width:61.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>40%,53%</span></p>
|  width=72 style='width:54.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>36%,54%</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>36%,54%</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>34%,54%</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>34%,54%</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>34.3%,53.8%</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>34.3%,53.8%</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>36.8%,54.9%</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>33.0%,54.4%</span></p>
|-  style='height:29.25pt'
|  width=83 style='width:62.0pt;border:solid white 1.0pt;border-top:none;  background:#E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' |
|  width=68 style='width:51.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>Throde valve opening rate</span></p>
|  width=81 style='width:61.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>17%</span></p>
|  width=72 style='width:54.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>12%</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>14%</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>14.7%</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>14.7%</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>14.7%</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>14.7%</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>16.2%</span></p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#E9EDF4;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' |
|-


|  width=83 style='width:62.0pt;border:solid white 1.0pt;border-top:none;  background:#D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:90.9pt' |
|  width=68 style='width:51.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:90.9pt' | <p class=MsoNormal><span lang=DA>Images </span></p>
|  width=81 style='width:61.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:90.9pt' | <p class=MsoNormal>Image1</p>
|  width=72 style='width:54.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:90.9pt' | <p class=MsoNormal>[[Specific_Process_Knowledge/Etch/ICP_Metal_Etcher/silicon_oxide/By_Peixiong/images_CF4#Images_stepper_6A4_feb262013_step9|Images]]</p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:90.9pt' | <p class=MsoNormal>Images3</p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:90.9pt' | <p class=MsoNormal>Images4</p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:90.9pt' | <p class=MsoNormal>Iamges5</p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:90.9pt' | <p class=MsoNormal>Images6</p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:90.9pt' | <p class=MsoNormal>Images7</p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:90.9pt' | <p class=MsoNormal>[[Specific_Process_Knowledge/Etch/ICP_Metal_Etcher/silicon_oxide/By_Peixiong/images_CF4#Images_Stepper_6A5_feb272013|Images]]</p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:90.9pt' |
|-
|  width=83 style='width:62.0pt;border:solid white 1.0pt;border-top:none;  background:#D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:90.9pt' |
|  width=68 style='width:51.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:90.9pt' | <p class=MsoNormal><span lang=DA>Comments </span></p>
|  width=81 style='width:61.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:90.9pt' | <p class=MsoNormal>Profile Very good, 2min etch SiO3 350nm in wafer center,
310nm in wafer, resist etched 260nm</p>
|  width=72 style='width:54.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:90.9pt' | <p class=MsoNormal>Profile Very good, 2min etch SiO3 350nm in wafer center,
310nm in wafer, resist etched 260nm</p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:90.9pt' | <p class=MsoNormal>Profile Very good, 4min etch SiO3 480nm in wafer center,
Resist etched 100nm</p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:90.9pt' | <p class=MsoNormal>Profile Very good, 4min etch SiO3 480nm in wafer center,
Resist etched 100nm, side wall 85degree</p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:90.9pt' | <p class=MsoNormal>Profile Very good, 4min etch SiO3 480nm in wafer center,
Resist etched 100nm</p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:90.9pt' | <p class=MsoNormal>Plasma very stable on blank Si wafer</p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:90.9pt' | <p class=MsoNormal>Plasma not stable in apox wafer</p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:90.9pt' | <p class=MsoNormal>etched 500nm apox, resit 150n, slide wall  86degm</p>
|  width=79 style='width:59.0pt;border-top:none;border-left:none;border-bottom:  solid white 1.0pt;border-right:solid white 1.0pt;background:#D0D8E8;  padding:2.25pt 2.25pt 2.25pt 2.25pt;height:90.9pt' |
|}<p class=MsoNormal>&nbsp;</p>
==Part2==
{|  class=MsoNormalTable border=0 cellspacing=0 cellpadding=0 width=517 style='width:388.0pt;border-collapse:collapse'  style='height:36.0pt'
|  width=163 valign=top style='width:122.0pt;border:solid white 1.0pt;  border-bottom:solid white 3.0pt;background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;  height:36.0pt' | <p class=MsoNormal>ICP metal etch SiO2 by reist mask try</p>
|  width=192 valign=top style='width:144.0pt;border-top:solid white 1.0pt;  border-left:none;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;  background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:36.0pt' | <p class=MsoNormal><span lang=DA>stable plasma at 2.5mtorr</span></p>
|  width=163 valign=top style='width:122.0pt;border-top:solid white 1.0pt;  border-left:none;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;  background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:36.0pt' | <p class=MsoNormal><span lang=DA>stable plasma at 2.5mtorr</span></p>
|-  style='height:31.25pt'
|  width=163 valign=top style='width:122.0pt;border-top:none;border-left:  solid white 1.0pt;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;  background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:31.25pt' | <p class=MsoNormal><span lang=DA>Date</span></p>
|  width=192 valign=top style='width:144.0pt;border-top:none;border-left:  none;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;  background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:31.25pt' | <p class=MsoNormal><span lang=DA>Feb28204am</span></p>
|  width=163 valign=top style='width:122.0pt;border-top:none;border-left:  none;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;  background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:31.25pt' | <p class=MsoNormal><span lang=DA>March012013, 21</span></p>
|-  style='height:26.15pt'
|  width=163 valign=top style='width:122.0pt;border-top:none;border-left:  solid white 1.0pt;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;  background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:26.15pt' | <p class=MsoNormal><span lang=DA>Metal ICP  recipe</span></p>
|  width=192 valign=top style='width:144.0pt;border-top:none;border-left:  none;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;  background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:26.15pt' | <p class=MsoNormal><span lang=DA>pxSiO2try9</span></p>
|  width=163 valign=top style='width:122.0pt;border-top:none;border-left:  none;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;  background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:26.15pt' | <p class=MsoNormal><span lang=DA>pxSiO2try9</span></p>
|-  style='height:28.9pt'
|  width=163 style='width:122.0pt;border-top:none;border-left:solid white 1.0pt;  border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;background:  #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:28.9pt' | <p class=MsoNormal><span lang=DA>Wafer size and ID</span></p>
|  width=192 style='width:144.0pt;border-top:none;border-left:none;  border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;background:  #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:28.9pt' | <p class=MsoNormal><span lang=DA>6inch,</span></p><p class=MsoNormal><span lang=DA>6A6_feb272013</span></p>
|  width=163 style='width:122.0pt;border-top:none;border-left:none;  border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;background:  #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:28.9pt' | <p class=MsoNormal><span lang=DA>6inch,</span></p><p class=MsoNormal><span lang=DA>6A1_march012013</span></p>
|-  style='height:53.85pt'
|  width=163 style='width:122.0pt;border:solid white 1.0pt;border-top:none;  background:#D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:53.85pt' | <p class=MsoNormal><span lang=DA>Mask</span></p>
|  width=192 style='width:144.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:53.85pt' | <p class=MsoNormal>780nm resist on 62nmBarc on 490nm apox, first etch barc
20sec by Ox plasma</p>
|  width=163 style='width:122.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:53.85pt' | <p class=MsoNormal>780nm resist on 62nmBarc on 490nm apox, first etch barc
20sec by Ox plasma</p>
|-  style='height:25.4pt'
|  width=163 style='width:122.0pt;border:solid white 1.0pt;border-top:none;  background:#E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:25.4pt' | <p class=MsoNormal><span lang=DA>Etch time</span></p>
|  width=192 style='width:144.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:25.4pt' | <p class=MsoNormal><span lang=DA>5min</span></p>
|  width=163 style='width:122.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:25.4pt' | <p class=MsoNormal><span lang=DA>65min</span></p>
|-  style='height:25.4pt'
|  width=163 style='width:122.0pt;border:solid white 1.0pt;border-top:none;  background:#E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:25.4pt' | <p class=MsoNormal><span lang=DA>Pressure [mTorr] </span></p>
|  width=192 style='width:144.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:25.4pt' | <p class=MsoNormal><span lang=DA>2.5</span></p>
|  width=163 style='width:122.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:25.4pt' | <p class=MsoNormal><span lang=DA>2.5</span></p>
|-  style='height:25.4pt'
|  width=163 style='width:122.0pt;border:solid white 1.0pt;border-top:none;  background:#E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:25.4pt' | <p class=MsoNormal><span lang=DA>C4F8 flow [sccm] </span></p>
|  width=192 style='width:144.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:25.4pt' | <p class=MsoNormal><span lang=DA>8</span></p>
|  width=163 style='width:122.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:25.4pt' | <p class=MsoNormal><span lang=DA>8</span></p>
|-  style='height:25.4pt'
|  width=163 style='width:122.0pt;border:solid white 1.0pt;border-top:none;  background:#E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:25.4pt' | <p class=MsoNormal><span lang=DA>CF4 flow [sccm] </span></p>
|  width=192 style='width:144.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:25.4pt' | <p class=MsoNormal><span lang=DA>0</span></p>
|  width=163 style='width:122.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:25.4pt' | <p class=MsoNormal><span lang=DA>0</span></p>
|-  style='height:25.4pt'
|  width=163 style='width:122.0pt;border:solid white 1.0pt;border-top:none;  background:#E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:25.4pt' | <p class=MsoNormal><span lang=DA>H2 flow [sccm] </span></p>
|  width=192 style='width:144.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:25.4pt' | <p class=MsoNormal><span lang=DA>30</span></p>
|  width=163 style='width:122.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:25.4pt' | <p class=MsoNormal><span lang=DA>30</span></p>
|-  style='height:25.4pt'
|  width=163 style='width:122.0pt;border:solid white 1.0pt;border-top:none;  background:#E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:25.4pt' | <p class=MsoNormal><span lang=DA>CH4 flow [sccm] </span></p>
|  width=192 style='width:144.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:25.4pt' | <p class=MsoNormal><span lang=DA>0</span></p>
|  width=163 style='width:122.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:25.4pt' | <p class=MsoNormal><span lang=DA>0</span></p>
|-  style='height:25.4pt'
|  width=163 style='width:122.0pt;border:solid white 1.0pt;border-top:none;  background:#E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:25.4pt' | <p class=MsoNormal><span lang=DA>Coil Power [W] </span></p>
|  width=192 style='width:144.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:25.4pt' | <p class=MsoNormal><span lang=DA>800 reflect 8W</span></p>
|  width=163 style='width:122.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:25.4pt' | <p class=MsoNormal><span lang=DA>800 reflect 8W</span></p>
|-  style='height:25.4pt'
|  width=163 style='width:122.0pt;border:solid white 1.0pt;border-top:none;  background:#D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:25.4pt' | <p class=MsoNormal><span lang=DA>Platen Power [W] </span></p>
|  width=192 style='width:144.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:25.4pt' | <p class=MsoNormal><span lang=DA>150reflect 0.2w</span></p>
|  width=163 style='width:122.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:25.4pt' | <p class=MsoNormal><span lang=DA>150reflect 0.2w</span></p>
|-  style='height:28.9pt'
|  width=163 style='width:122.0pt;border:solid white 1.0pt;border-top:none;  background:#E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:28.9pt' | <p class=MsoNormal><span lang=DA>Platen temperature [<sup>o</sup>C] </span></p>
|  width=192 style='width:144.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:28.9pt' | <p class=MsoNormal><span lang=DA>20</span></p>
|  width=163 style='width:122.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:28.9pt' | <p class=MsoNormal><span lang=DA>20</span></p>
|-  style='height:25.4pt'
|  width=163 style='width:122.0pt;border:solid white 1.0pt;border-top:none;  background:#D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:25.4pt' | <p class=MsoNormal><span lang=DA>Coil match</span></p>
|  width=192 style='width:144.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:25.4pt' | <p class=MsoNormal><span lang=DA>68.87%,23.1%</span></p>
|  width=163 style='width:122.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:25.4pt' | <p class=MsoNormal><span lang=DA>68.87%,23.1%</span></p>
|-  style='height:25.4pt'
|  width=163 style='width:122.0pt;border:solid white 1.0pt;border-top:none;  background:#D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:25.4pt' | <p class=MsoNormal><span lang=DA>Platen Match</span></p>
|  width=192 style='width:144.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:25.4pt' | <p class=MsoNormal><span lang=DA>33.0%,54.4%</span></p>
|  width=163 style='width:122.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:25.4pt' | <p class=MsoNormal><span lang=DA>33.0%,54.4%</span></p>
|-  style='height:45.6pt'
|  width=163 style='width:122.0pt;border:solid white 1.0pt;border-top:none;  background:#E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:45.6pt' | <p class=MsoNormal><span lang=DA>Throde valve opening rate</span></p>
|  width=192 style='width:144.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:45.6pt' |
|  width=163 style='width:122.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:45.6pt' | <p class=MsoNormal>10.8% to 11.7%, pressure 2.11 to 2.40, not stable</p>
|-  style='height:25.4pt'
|  width=163 style='width:122.0pt;border:solid white 1.0pt;border-top:none;  background:#D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:25.4pt' | <p class=MsoNormal><span lang=DA>Comments </span></p>
|  width=192 style='width:144.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:25.4pt' |
|  width=163 style='width:122.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:25.4pt' | <p class=MsoNormal><span lang=DA>SiO2 width 230nm</span></p>
|}<p class=MsoNormal><span lang=DA>&nbsp;</span></p>
=With CF4 and H2 chemistry by ''Peixiong Shi, DTU Nanolab''=
==Part 1==
<!--
<!--
  /* Font Definitions */
  /* Font Definitions */
Line 645: Line 976:
</div>
</div>


==Part 2==


==jsdlfiaj==
<div class=WordSection1>
{|  class=MsoNormalTable border=0 cellspacing=0 cellpadding=0 width=748 style='width:561.0pt;border-collapse:collapse'  style='height:29.25pt'
|  width=136 valign=top style='width:102.0pt;border:solid white 1.0pt;  border-bottom:solid white 3.0pt;background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;  height:29.25pt' |
|  width=136 valign=top style='width:102.0pt;border-top:solid white 1.0pt;  border-left:none;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;  background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>bad</span></p>
|  width=108 valign=top style='width:81.0pt;border-top:solid white 1.0pt;  border-left:none;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;  background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>bad</span></p>
|  width=119 valign=top style='width:89.0pt;border-top:solid white 1.0pt;  border-left:none;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;  background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>bad</span></p>
|  width=121 valign=top style='width:91.0pt;border-top:solid white 1.0pt;  border-left:none;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;  background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>Very good</span></p>
|  width=128 valign=top style='width:96.0pt;border-top:solid white 1.0pt;  border-left:none;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;  background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:29.25pt' |
|-  style='height:29.25pt'
|  width=136 valign=top style='width:102.0pt;border-top:none;border-left:  solid white 1.0pt;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;  background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:29.25pt' | <p class=MsoNormal>ICP metal etch SiO2 by reist mask try</p>
|  width=136 valign=top style='width:102.0pt;border-top:none;border-left:  none;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;  background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>Date</span></p>
|  width=108 valign=top style='width:81.0pt;border-top:none;border-left:  none;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;  background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>Feb252013</span></p>
|  width=119 valign=top style='width:89.0pt;border-top:none;border-left:  none;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;  background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>Feb252013</span></p>
|  width=121 valign=top style='width:91.0pt;border-top:none;border-left:  none;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;  background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>Feb262013</span></p>
|  width=128 valign=top style='width:96.0pt;border-top:none;border-left:  none;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;  background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:29.25pt' |
|-  style='height:29.25pt'
|  width=136 valign=top style='width:102.0pt;border-top:none;border-left:  solid white 1.0pt;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;  background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:29.25pt' |
|  width=136 valign=top style='width:102.0pt;border-top:none;border-left:  none;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;  background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>Metal ICP  recipe</span></p>
|  width=108 valign=top style='width:81.0pt;border-top:none;border-left:  none;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;  background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>pxSiO2try3</span></p>
|  width=119 valign=top style='width:89.0pt;border-top:none;border-left:  none;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;  background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>pxSiO2try4</span></p>
|  width=121 valign=top style='width:91.0pt;border-top:none;border-left:  none;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;  background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>pxSiO2try5</span></p>
|  width=128 valign=top style='width:96.0pt;border-top:none;border-left:  none;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;  background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:29.25pt' |
|-  style='height:29.25pt'
|  width=136 style='width:102.0pt;border-top:none;border-left:solid white 1.0pt;  border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;background:  #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' |
|  width=136 style='width:102.0pt;border-top:none;border-left:none;  border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;background:  #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>Wafer size and ID</span></p>
|  width=108 style='width:81.0pt;border-top:none;border-left:none;  border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;background:  #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>6inch,</span></p><p class=MsoNormal><span lang=DA>6A1_feb252013</span></p>
|  width=119 style='width:89.0pt;border-top:none;border-left:none;  border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;background:  #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>6inch,</span></p><p class=MsoNormal><span lang=DA>6A6_feb252013</span></p>
|  width=121 style='width:91.0pt;border-top:none;border-left:none;  border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;background:  #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>6inch,</span></p><p class=MsoNormal><span lang=DA>6A1_feb252013</span></p>
|  width=128 style='width:96.0pt;border-top:none;border-left:none;  border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;background:  #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' |
|-  style='height:42.9pt'
|  width=136 style='width:102.0pt;border:solid white 1.0pt;border-top:none;  background:#D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:42.9pt' |
|  width=136 style='width:102.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:42.9pt' | <p class=MsoNormal><span lang=DA>Mask</span></p>
|  width=108 style='width:81.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:42.9pt' | <p class=MsoNormal>980nm resist resist on 62nmBarc on 1190nm apox</p>
|  width=119 style='width:89.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:42.9pt' | <p class=MsoNormal>780nm resist on 62nmBarc on 492nm apox, first etch barc
20sec by Ox plasma</p>
|  width=121 style='width:91.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:42.9pt' | <p class=MsoNormal>440nm resist on 62nmBarc on 1800nm apox, first etch barc
20sec by Ox plasma</p>
|  width=128 style='width:96.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:42.9pt' |
|-  style='height:29.25pt'
|  width=136 style='width:102.0pt;border:solid white 1.0pt;border-top:none;  background:#E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' |
|  width=136 style='width:102.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>Etch time</span></p>
|  width=108 style='width:81.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>3min</span></p>
|  width=119 style='width:89.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>3min</span></p>
|  width=121 style='width:91.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>2min</span></p>
|  width=128 style='width:96.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' |
|-  style='height:29.25pt'
|  width=136 style='width:102.0pt;border:solid white 1.0pt;border-top:none;  background:#E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' |
|  width=136 style='width:102.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>Pressure [mTorr] </span></p>
|  width=108 style='width:81.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>15</span></p>
|  width=119 style='width:89.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>8</span></p>
|  width=121 style='width:91.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>6</span></p>
|  width=128 style='width:96.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' |
|-  style='height:29.25pt'
|  width=136 style='width:102.0pt;border:solid white 1.0pt;border-top:none;  background:#E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' |
|  width=136 style='width:102.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>C4F8 flow [sccm] </span></p>
|  width=108 style='width:81.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>0</span></p>
|  width=119 style='width:89.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>0</span></p>
|  width=121 style='width:91.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>0</span></p>
|  width=128 style='width:96.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' |
|-  style='height:29.25pt'
|  width=136 style='width:102.0pt;border:solid white 1.0pt;border-top:none;  background:#E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' |
|  width=136 style='width:102.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>CF4 flow [sccm] </span></p>
|  width=108 style='width:81.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>40</span></p>
|  width=119 style='width:89.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>40</span></p>
|  width=121 style='width:91.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>40</span></p>
|  width=128 style='width:96.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' |
|-  style='height:29.25pt'
|  width=136 style='width:102.0pt;border:solid white 1.0pt;border-top:none;  background:#E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' |
|  width=136 style='width:102.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>H2 flow [sccm] </span></p>
|  width=108 style='width:81.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>30</span></p>
|  width=119 style='width:89.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>30</span></p>
|  width=121 style='width:91.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>30</span></p>
|  width=128 style='width:96.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' |
|-  style='height:29.25pt'
|  width=136 style='width:102.0pt;border:solid white 1.0pt;border-top:none;  background:#E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' |
|  width=136 style='width:102.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>Coil Power [W] </span></p>
|  width=108 style='width:81.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>800</span></p>
|  width=119 style='width:89.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>800</span></p>
|  width=121 style='width:91.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>800</span></p>
|  width=128 style='width:96.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' |
|-  style='height:29.25pt'
|  width=136 style='width:102.0pt;border:solid white 1.0pt;border-top:none;  background:#D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' |
|  width=136 style='width:102.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>Platen Power [W] </span></p>
|  width=108 style='width:81.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>200 </span></p>
|  width=119 style='width:89.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>200 </span></p>
|  width=121 style='width:91.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>100</span></p>
|  width=128 style='width:96.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' |
|-  style='height:29.25pt'
|  width=136 style='width:102.0pt;border:solid white 1.0pt;border-top:none;  background:#E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' |
|  width=136 style='width:102.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>Platen temperature [<sup>o</sup>C] </span></p>
|  width=108 style='width:81.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>20 </span></p>
|  width=119 style='width:89.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>20 </span></p>
|  width=121 style='width:91.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>20</span></p>
|  width=128 style='width:96.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' |
|-  style='height:29.25pt'
|  width=136 style='width:102.0pt;border:solid white 1.0pt;border-top:none;  background:#D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' |
|  width=136 style='width:102.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>Coil match</span></p>
|  width=108 style='width:81.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>50%, 30%</span></p>
|  width=119 style='width:89.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>59%, 27%</span></p>
|  width=121 style='width:91.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>60%,27%</span></p>
|  width=128 style='width:96.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' |
|-  style='height:29.25pt'
|  width=136 style='width:102.0pt;border:solid white 1.0pt;border-top:none;  background:#D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' |
|  width=136 style='width:102.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>Platen Match</span></p>
|  width=108 style='width:81.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>50%, 57%</span></p>
|  width=119 style='width:89.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>44%, 56%</span></p>
|  width=121 style='width:91.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>40%,53%</span></p>
|  width=128 style='width:96.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' |
|-  style='height:29.25pt'
|  width=136 style='width:102.0pt;border:solid white 1.0pt;border-top:none;  background:#E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' |
|  width=136 style='width:102.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>Throde valve opening rate</span></p>
|  width=108 style='width:81.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>10%</span></p>
|  width=119 style='width:89.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>13.6%</span></p>
|  width=121 style='width:91.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' | <p class=MsoNormal><span lang=DA>17%</span></p>
|  width=128 style='width:96.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt' |
|-  style='height:52.5pt'
|  width=136 style='width:102.0pt;border:solid white 1.0pt;border-top:none;  background:#D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:52.5pt' |
|  width=136 style='width:102.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:52.5pt' | <p class=MsoNormal><span lang=DA>Images </span></p>
|  width=108 style='width:81.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:52.5pt' | <p class=MsoNormal></p>
|  width=119 style='width:89.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:52.5pt' | <p class=MsoNormal>Images 2</p>
|  width=121 style='width:91.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background:  #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:52.5pt' | <p class=MsoNormal>[[Specific_Process_Knowledge/Etch/ICP_Metal_Etcher/silicon_oxide/By_Peixiong/images_CF4#Images_stepper_6A1_feb262013_step9|Images]]</p>
|  width=128 valign=top style='width:96.0pt;border-top:none;border-left:  none;border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;  background:#D0D8E8;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:52.5pt' | <p class=MsoNormal></p>


<html xmlns:v="urn:schemas-microsoft-com:vml"
|- style='height:52.5pt'
xmlns:o="urn:schemas-microsoft-com:office:office"
|  width=136 style='width:102.0pt;border:solid white 1.0pt;border-top:none;  background:#D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:52.5pt' |
xmlns:w="urn:schemas-microsoft-com:office:word"
|  width=136 style='width:102.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background: #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:52.5pt' | <p class=MsoNormal><span lang=DA>Comments </span></p>
xmlns:m="http://schemas.microsoft.com/office/2004/12/omml"
|  width=108 style='width:81.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background: #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:52.5pt' | <p class=MsoNormal>Apox etch 550nm for 3min, side wall angle 71degree</p>
xmlns="http://www.w3.org/TR/REC-html40"><head><meta http-equiv=Content-Type content="text/html; charset=windows-1252"><meta name=ProgId content=Word.Document><meta name=Generator content="Microsoft Word 14"><meta name=Originator content="Microsoft Word 14"><link rel=File-List href="px%20ch4%202_files/filelist.xml"><!--[if gte mso 9]><xml><o:DocumentProperties><o:Author>Berit Herstrøm</o:Author><o:LastAuthor>Berit Herstrøm</o:LastAuthor><o:Revision>1</o:Revision><o:TotalTime>0</o:TotalTime><o:Created>2016-05-02T12:39:00Z</o:Created><o:LastSaved>2016-05-02T12:39:00Z</o:LastSaved><o:Pages>2</o:Pages><o:Words>168</o:Words><o:Characters>963</o:Characters><o:Company>DTU</o:Company><o:Lines>8</o:Lines><o:Paragraphs>2</o:Paragraphs><o:CharactersWithSpaces>1129</o:CharactersWithSpaces><o:Version>14.00</o:Version></o:DocumentProperties><o:OfficeDocumentSettings><o:AllowPNG/></o:OfficeDocumentSettings></xml><![endif]--><link rel=themeData href="px%20ch4%202_files/themedata.thmx"><link rel=colorSchemeMapping href="px%20ch4%202_files/colorschememapping.xml"><!--[if gte mso 9]><xml><w:WordDocument><w:SpellingState>Clean</w:SpellingState><w:GrammarState>Clean</w:GrammarState><w:TrackMoves/><w:TrackFormatting/><w:HyphenationZone>21</w:HyphenationZone><w:PunctuationKerning/><w:ValidateAgainstSchemas/><w:SaveIfXMLInvalid>false</w:SaveIfXMLInvalid><w:IgnoreMixedContent>false</w:IgnoreMixedContent><w:AlwaysShowPlaceholderText>false</w:AlwaysShowPlaceholderText><w:DoNotPromoteQF/><w:LidThemeOther>DA</w:LidThemeOther><w:LidThemeAsian>X-NONE</w:LidThemeAsian><w:LidThemeComplexScript>X-NONE</w:LidThemeComplexScript><w:Compatibility><w:BreakWrappedTables/><w:SnapToGridInCell/><w:WrapTextWithPunct/><w:UseAsianBreakRules/><w:DontGrowAutofit/><w:SplitPgBreakAndParaMark/><w:EnableOpenTypeKerning/><w:DontFlipMirrorIndents/><w:OverrideTableStyleHps/></w:Compatibility><m:mathPr><m:mathFont m:val="Cambria Math"/><m:brkBin m:val="before"/><m:brkBinSub m:val="--"/><m:smallFrac m:val="off"/><m:dispDef/><m:lMargin m:val="0"/><m:rMargin m:val="0"/><m:defJc m:val="centerGroup"/><m:wrapIndent m:val="1440"/><m:intLim m:val="subSup"/><m:naryLim m:val="undOvr"/></m:mathPr></w:WordDocument></xml><![endif]--><!--[if gte mso 9]><xml><w:LatentStyles DefLockedState="false" DefUnhideWhenUsed="true"
|  width=119 style='width:89.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background: #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:52.5pt' | <p class=MsoNormal>Too much polymer, etch Si too much</p><p class=MsoNormal>Etch through 500nm apox, then etch Si 180nm,</p>
DefSemiHidden="true" DefQFormat="false" DefPriority="99"
|  width=121 style='width:91.0pt;border-top:none;border-left:none;  border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;background: #D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;height:52.5pt' | <p class=MsoNormal>Profile Very good, 2min etch SiO3 350nm in wafer center,
LatentStyleCount="267"><w:LsdException Locked="false" Priority="0" SemiHidden="false"
310nm in wafer, resist etched 260nm</p>
UnhideWhenUsed="false" QFormat="true" Name="Normal"/><w:LsdException Locked="false" Priority="9" SemiHidden="false"
|  width=128 valign=top style='width:96.0pt;border-top:none;border-left: none;border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;  background:#D0D8E8;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:52.5pt' | <p class=MsoNormal>Low pressure gives better profile, less polymer, however,
UnhideWhenUsed="false" QFormat="true" Name="heading 1"/><w:LsdException Locked="false" Priority="9" QFormat="true" Name="heading 2"/><w:LsdException Locked="false" Priority="9" QFormat="true" Name="heading 3"/><w:LsdException Locked="false" Priority="9" QFormat="true" Name="heading 4"/><w:LsdException Locked="false" Priority="9" QFormat="true" Name="heading 5"/><w:LsdException Locked="false" Priority="9" QFormat="true" Name="heading 6"/><w:LsdException Locked="false" Priority="9" QFormat="true" Name="heading 7"/><w:LsdException Locked="false" Priority="9" QFormat="true" Name="heading 8"/><w:LsdException Locked="false" Priority="9" QFormat="true" Name="heading 9"/><w:LsdException Locked="false" Priority="39" Name="toc 1"/><w:LsdException Locked="false" Priority="39" Name="toc 2"/><w:LsdException Locked="false" Priority="39" Name="toc 3"/><w:LsdException Locked="false" Priority="39" Name="toc 4"/><w:LsdException Locked="false" Priority="39" Name="toc 5"/><w:LsdException Locked="false" Priority="39" Name="toc 6"/><w:LsdException Locked="false" Priority="39" Name="toc 7"/><w:LsdException Locked="false" Priority="39" Name="toc 8"/><w:LsdException Locked="false" Priority="39" Name="toc 9"/><w:LsdException Locked="false" Priority="35" QFormat="true" Name="caption"/><w:LsdException Locked="false" Priority="10" SemiHidden="false"
CF4 etch Si too quick</p>
UnhideWhenUsed="false" QFormat="true" Name="Title"/><w:LsdException Locked="false" Priority="1" Name="Default Paragraph Font"/><w:LsdException Locked="false" Priority="11" SemiHidden="false"
|}<p class=MsoNormal>&nbsp;</p></div>
UnhideWhenUsed="false" QFormat="true" Name="Subtitle"/><w:LsdException Locked="false" Priority="22" SemiHidden="false"
UnhideWhenUsed="false" QFormat="true" Name="Strong"/><w:LsdException Locked="false" Priority="20" SemiHidden="false"
UnhideWhenUsed="false" QFormat="true" Name="Emphasis"/><w:LsdException Locked="false" Priority="59" SemiHidden="false"
UnhideWhenUsed="false" Name="Table Grid"/><w:LsdException Locked="false" UnhideWhenUsed="false" Name="Placeholder Text"/><w:LsdException Locked="false" Priority="1" SemiHidden="false"
UnhideWhenUsed="false" QFormat="true" Name="No Spacing"/><w:LsdException Locked="false" Priority="60" SemiHidden="false"
UnhideWhenUsed="false" Name="Light Shading"/><w:LsdException Locked="false" Priority="61" SemiHidden="false"
UnhideWhenUsed="false" Name="Light List"/><w:LsdException Locked="false" Priority="62" SemiHidden="false"
UnhideWhenUsed="false" Name="Light Grid"/><w:LsdException Locked="false" Priority="63" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium Shading 1"/><w:LsdException Locked="false" Priority="64" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium Shading 2"/><w:LsdException Locked="false" Priority="65" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium List 1"/><w:LsdException Locked="false" Priority="66" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium List 2"/><w:LsdException Locked="false" Priority="67" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium Grid 1"/><w:LsdException Locked="false" Priority="68" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium Grid 2"/><w:LsdException Locked="false" Priority="69" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium Grid 3"/><w:LsdException Locked="false" Priority="70" SemiHidden="false"
UnhideWhenUsed="false" Name="Dark List"/><w:LsdException Locked="false" Priority="71" SemiHidden="false"
UnhideWhenUsed="false" Name="Colorful Shading"/><w:LsdException Locked="false" Priority="72" SemiHidden="false"
UnhideWhenUsed="false" Name="Colorful List"/><w:LsdException Locked="false" Priority="73" SemiHidden="false"
UnhideWhenUsed="false" Name="Colorful Grid"/><w:LsdException Locked="false" Priority="60" SemiHidden="false"
UnhideWhenUsed="false" Name="Light Shading Accent 1"/><w:LsdException Locked="false" Priority="61" SemiHidden="false"
UnhideWhenUsed="false" Name="Light List Accent 1"/><w:LsdException Locked="false" Priority="62" SemiHidden="false"
UnhideWhenUsed="false" Name="Light Grid Accent 1"/><w:LsdException Locked="false" Priority="63" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium Shading 1 Accent 1"/><w:LsdException Locked="false" Priority="64" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium Shading 2 Accent 1"/><w:LsdException Locked="false" Priority="65" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium List 1 Accent 1"/><w:LsdException Locked="false" UnhideWhenUsed="false" Name="Revision"/><w:LsdException Locked="false" Priority="34" SemiHidden="false"
UnhideWhenUsed="false" QFormat="true" Name="List Paragraph"/><w:LsdException Locked="false" Priority="29" SemiHidden="false"
UnhideWhenUsed="false" QFormat="true" Name="Quote"/><w:LsdException Locked="false" Priority="30" SemiHidden="false"
UnhideWhenUsed="false" QFormat="true" Name="Intense Quote"/><w:LsdException Locked="false" Priority="66" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium List 2 Accent 1"/><w:LsdException Locked="false" Priority="67" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium Grid 1 Accent 1"/><w:LsdException Locked="false" Priority="68" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium Grid 2 Accent 1"/><w:LsdException Locked="false" Priority="69" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium Grid 3 Accent 1"/><w:LsdException Locked="false" Priority="70" SemiHidden="false"
UnhideWhenUsed="false" Name="Dark List Accent 1"/><w:LsdException Locked="false" Priority="71" SemiHidden="false"
UnhideWhenUsed="false" Name="Colorful Shading Accent 1"/><w:LsdException Locked="false" Priority="72" SemiHidden="false"
UnhideWhenUsed="false" Name="Colorful List Accent 1"/><w:LsdException Locked="false" Priority="73" SemiHidden="false"
UnhideWhenUsed="false" Name="Colorful Grid Accent 1"/><w:LsdException Locked="false" Priority="60" SemiHidden="false"
UnhideWhenUsed="false" Name="Light Shading Accent 2"/><w:LsdException Locked="false" Priority="61" SemiHidden="false"
UnhideWhenUsed="false" Name="Light List Accent 2"/><w:LsdException Locked="false" Priority="62" SemiHidden="false"
UnhideWhenUsed="false" Name="Light Grid Accent 2"/><w:LsdException Locked="false" Priority="63" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium Shading 1 Accent 2"/><w:LsdException Locked="false" Priority="64" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium Shading 2 Accent 2"/><w:LsdException Locked="false" Priority="65" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium List 1 Accent 2"/><w:LsdException Locked="false" Priority="66" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium List 2 Accent 2"/><w:LsdException Locked="false" Priority="67" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium Grid 1 Accent 2"/><w:LsdException Locked="false" Priority="68" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium Grid 2 Accent 2"/><w:LsdException Locked="false" Priority="69" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium Grid 3 Accent 2"/><w:LsdException Locked="false" Priority="70" SemiHidden="false"
UnhideWhenUsed="false" Name="Dark List Accent 2"/><w:LsdException Locked="false" Priority="71" SemiHidden="false"
UnhideWhenUsed="false" Name="Colorful Shading Accent 2"/><w:LsdException Locked="false" Priority="72" SemiHidden="false"
UnhideWhenUsed="false" Name="Colorful List Accent 2"/><w:LsdException Locked="false" Priority="73" SemiHidden="false"
UnhideWhenUsed="false" Name="Colorful Grid Accent 2"/><w:LsdException Locked="false" Priority="60" SemiHidden="false"
UnhideWhenUsed="false" Name="Light Shading Accent 3"/><w:LsdException Locked="false" Priority="61" SemiHidden="false"
UnhideWhenUsed="false" Name="Light List Accent 3"/><w:LsdException Locked="false" Priority="62" SemiHidden="false"
UnhideWhenUsed="false" Name="Light Grid Accent 3"/><w:LsdException Locked="false" Priority="63" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium Shading 1 Accent 3"/><w:LsdException Locked="false" Priority="64" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium Shading 2 Accent 3"/><w:LsdException Locked="false" Priority="65" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium List 1 Accent 3"/><w:LsdException Locked="false" Priority="66" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium List 2 Accent 3"/><w:LsdException Locked="false" Priority="67" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium Grid 1 Accent 3"/><w:LsdException Locked="false" Priority="68" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium Grid 2 Accent 3"/><w:LsdException Locked="false" Priority="69" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium Grid 3 Accent 3"/><w:LsdException Locked="false" Priority="70" SemiHidden="false"
UnhideWhenUsed="false" Name="Dark List Accent 3"/><w:LsdException Locked="false" Priority="71" SemiHidden="false"
UnhideWhenUsed="false" Name="Colorful Shading Accent 3"/><w:LsdException Locked="false" Priority="72" SemiHidden="false"
UnhideWhenUsed="false" Name="Colorful List Accent 3"/><w:LsdException Locked="false" Priority="73" SemiHidden="false"
UnhideWhenUsed="false" Name="Colorful Grid Accent 3"/><w:LsdException Locked="false" Priority="60" SemiHidden="false"
UnhideWhenUsed="false" Name="Light Shading Accent 4"/><w:LsdException Locked="false" Priority="61" SemiHidden="false"
UnhideWhenUsed="false" Name="Light List Accent 4"/><w:LsdException Locked="false" Priority="62" SemiHidden="false"
UnhideWhenUsed="false" Name="Light Grid Accent 4"/><w:LsdException Locked="false" Priority="63" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium Shading 1 Accent 4"/><w:LsdException Locked="false" Priority="64" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium Shading 2 Accent 4"/><w:LsdException Locked="false" Priority="65" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium List 1 Accent 4"/><w:LsdException Locked="false" Priority="66" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium List 2 Accent 4"/><w:LsdException Locked="false" Priority="67" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium Grid 1 Accent 4"/><w:LsdException Locked="false" Priority="68" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium Grid 2 Accent 4"/><w:LsdException Locked="false" Priority="69" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium Grid 3 Accent 4"/><w:LsdException Locked="false" Priority="70" SemiHidden="false"
UnhideWhenUsed="false" Name="Dark List Accent 4"/><w:LsdException Locked="false" Priority="71" SemiHidden="false"
UnhideWhenUsed="false" Name="Colorful Shading Accent 4"/><w:LsdException Locked="false" Priority="72" SemiHidden="false"
UnhideWhenUsed="false" Name="Colorful List Accent 4"/><w:LsdException Locked="false" Priority="73" SemiHidden="false"
UnhideWhenUsed="false" Name="Colorful Grid Accent 4"/><w:LsdException Locked="false" Priority="60" SemiHidden="false"
UnhideWhenUsed="false" Name="Light Shading Accent 5"/><w:LsdException Locked="false" Priority="61" SemiHidden="false"
UnhideWhenUsed="false" Name="Light List Accent 5"/><w:LsdException Locked="false" Priority="62" SemiHidden="false"
UnhideWhenUsed="false" Name="Light Grid Accent 5"/><w:LsdException Locked="false" Priority="63" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium Shading 1 Accent 5"/><w:LsdException Locked="false" Priority="64" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium Shading 2 Accent 5"/><w:LsdException Locked="false" Priority="65" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium List 1 Accent 5"/><w:LsdException Locked="false" Priority="66" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium List 2 Accent 5"/><w:LsdException Locked="false" Priority="67" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium Grid 1 Accent 5"/><w:LsdException Locked="false" Priority="68" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium Grid 2 Accent 5"/><w:LsdException Locked="false" Priority="69" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium Grid 3 Accent 5"/><w:LsdException Locked="false" Priority="70" SemiHidden="false"
UnhideWhenUsed="false" Name="Dark List Accent 5"/><w:LsdException Locked="false" Priority="71" SemiHidden="false"
UnhideWhenUsed="false" Name="Colorful Shading Accent 5"/><w:LsdException Locked="false" Priority="72" SemiHidden="false"
UnhideWhenUsed="false" Name="Colorful List Accent 5"/><w:LsdException Locked="false" Priority="73" SemiHidden="false"
UnhideWhenUsed="false" Name="Colorful Grid Accent 5"/><w:LsdException Locked="false" Priority="60" SemiHidden="false"
UnhideWhenUsed="false" Name="Light Shading Accent 6"/><w:LsdException Locked="false" Priority="61" SemiHidden="false"
UnhideWhenUsed="false" Name="Light List Accent 6"/><w:LsdException Locked="false" Priority="62" SemiHidden="false"
UnhideWhenUsed="false" Name="Light Grid Accent 6"/><w:LsdException Locked="false" Priority="63" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium Shading 1 Accent 6"/><w:LsdException Locked="false" Priority="64" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium Shading 2 Accent 6"/><w:LsdException Locked="false" Priority="65" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium List 1 Accent 6"/><w:LsdException Locked="false" Priority="66" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium List 2 Accent 6"/><w:LsdException Locked="false" Priority="67" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium Grid 1 Accent 6"/><w:LsdException Locked="false" Priority="68" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium Grid 2 Accent 6"/><w:LsdException Locked="false" Priority="69" SemiHidden="false"
UnhideWhenUsed="false" Name="Medium Grid 3 Accent 6"/><w:LsdException Locked="false" Priority="70" SemiHidden="false"
UnhideWhenUsed="false" Name="Dark List Accent 6"/><w:LsdException Locked="false" Priority="71" SemiHidden="false"
UnhideWhenUsed="false" Name="Colorful Shading Accent 6"/><w:LsdException Locked="false" Priority="72" SemiHidden="false"
UnhideWhenUsed="false" Name="Colorful List Accent 6"/><w:LsdException Locked="false" Priority="73" SemiHidden="false"
UnhideWhenUsed="false" Name="Colorful Grid Accent 6"/><w:LsdException Locked="false" Priority="19" SemiHidden="false"
UnhideWhenUsed="false" QFormat="true" Name="Subtle Emphasis"/><w:LsdException Locked="false" Priority="21" SemiHidden="false"
UnhideWhenUsed="false" QFormat="true" Name="Intense Emphasis"/><w:LsdException Locked="false" Priority="31" SemiHidden="false"
UnhideWhenUsed="false" QFormat="true" Name="Subtle Reference"/><w:LsdException Locked="false" Priority="32" SemiHidden="false"
UnhideWhenUsed="false" QFormat="true" Name="Intense Reference"/><w:LsdException Locked="false" Priority="33" SemiHidden="false"
UnhideWhenUsed="false" QFormat="true" Name="Book Title"/><w:LsdException Locked="false" Priority="37" Name="Bibliography"/><w:LsdException Locked="false" Priority="39" QFormat="true" Name="TOC Heading"/></w:LatentStyles></xml><![endif]--><style><!--
/* Font Definitions */
@font-face
{font-family:Calibri;
panose-1:2 15 5 2 2 2 4 3 2 4;
mso-font-charset:0;
mso-generic-font-family:swiss;
mso-font-pitch:variable;
mso-font-signature:-536870145 1073786111 1 0 415 0;}
/* Style Definitions */
p.MsoNormal, li.MsoNormal, div.MsoNormal
{mso-style-unhide:no;
mso-style-qformat:yes;
mso-style-parent:"";
margin-top:0cm;
margin-right:0cm;
margin-bottom:10.0pt;
margin-left:0cm;
line-height:115%;
mso-pagination:widow-orphan;
font-size:11.0pt;
font-family:"Calibri","sans-serif";
mso-ascii-font-family:Calibri;
mso-ascii-theme-font:minor-latin;
mso-fareast-font-family:Calibri;
mso-fareast-theme-font:minor-latin;
mso-hansi-font-family:Calibri;
mso-hansi-theme-font:minor-latin;
mso-bidi-font-family:"Times New Roman";
mso-bidi-theme-font:minor-bidi;
mso-ansi-language:DA;}
span.SpellE
{mso-style-name:"";
mso-spl-e:yes;}
span.GramE
{mso-style-name:"";
mso-gram-e:yes;}
.MsoChpDefault
{mso-style-type:export-only;
mso-default-props:yes;
font-family:"Calibri","sans-serif";
mso-ascii-font-family:Calibri;
mso-ascii-theme-font:minor-latin;
mso-fareast-font-family:Calibri;
mso-fareast-theme-font:minor-latin;
mso-hansi-font-family:Calibri;
mso-hansi-theme-font:minor-latin;
mso-bidi-font-family:"Times New Roman";
mso-bidi-theme-font:minor-bidi;
mso-ansi-language:DA;}
.MsoPapDefault
{mso-style-type:export-only;
margin-bottom:10.0pt;
line-height:115%;}
@page WordSection1
{size:841.9pt 595.3pt;
mso-page-orientation:landscape;
margin:2.0cm 3.0cm 2.0cm 3.0cm;
mso-header-margin:35.4pt;
mso-footer-margin:35.4pt;
mso-paper-source:0;}
div.WordSection1
{page:WordSection1;}
--></style><!--[if gte mso 10]><style>
/* Style Definitions */
table.MsoNormalTable
{mso-style-name:"Table Normal";
mso-tstyle-rowband-size:0;
mso-tstyle-colband-size:0;
mso-style-noshow:yes;
mso-style-priority:99;
mso-style-parent:"";
mso-padding-alt:0cm 5.4pt 0cm 5.4pt;
mso-para-margin-top:0cm;
mso-para-margin-right:0cm;
mso-para-margin-bottom:10.0pt;
mso-para-margin-left:0cm;
line-height:115%;
mso-pagination:widow-orphan;
font-size:11.0pt;
font-family:"Calibri","sans-serif";
mso-ascii-font-family:Calibri;
mso-ascii-theme-font:minor-latin;
mso-hansi-font-family:Calibri;
mso-hansi-theme-font:minor-latin;
mso-ansi-language:DA;}
</style><![endif]--><!--[if gte mso 9]><xml><o:shapedefaults v:ext="edit" spidmax="1026"/></xml><![endif]--><!--[if gte mso 9]><xml><o:shapelayout v:ext="edit"><o:idmap v:ext="edit" data="1"/></o:shapelayout></xml><![endif]--></head><body lang=EN-US style='tab-interval:65.2pt'><div class=WordSection1>
{| class=MsoNormalTable border=0 cellspacing=0 cellpadding=0 width=748  style='width:561.0pt;border-collapse:collapse;mso-yfti-tbllook:1536;  mso-padding-alt:0cm 0cm 0cm 0cm'
|- style='mso-yfti-irow:0;mso-yfti-firstrow:yes;height:29.25pt'<td width=136 valign=top style='width:102.0pt;border:solid white 1.0pt;
border-bottom:solid white 3.0pt;background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;
height:29.25pt'><td width=136 valign=top style='width:102.0pt;border-top:solid white 1.0pt;
border-left:none;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;
mso-border-left-alt:solid white 1.0pt;background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;
height:29.25pt'><p class=MsoNormal><span lang=DA>bad</span><span style='mso-ansi-language:
EN-US'><o:p></o:p></span><td width=108 valign=top style='width:81.0pt;border-top:solid white 1.0pt;
border-left:none;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;
mso-border-left-alt:solid white 1.0pt;background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;
height:29.25pt'><p class=MsoNormal><span lang=DA>bad</span><span style='mso-ansi-language:
EN-US'><o:p></o:p></span><td width=119 valign=top style='width:89.0pt;border-top:solid white 1.0pt;
border-left:none;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;
mso-border-left-alt:solid white 1.0pt;background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;
height:29.25pt'><p class=MsoNormal><span lang=DA>bad</span><span style='mso-ansi-language:
EN-US'><o:p></o:p></span><td width=121 valign=top style='width:91.0pt;border-top:solid white 1.0pt;
border-left:none;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;
mso-border-left-alt:solid white 1.0pt;background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;
height:29.25pt'><p class=MsoNormal><span class=SpellE><span lang=DA>Very</span></span><span
lang=DA><span class=SpellE>good</span></span><span style='mso-ansi-language:
EN-US'><o:p></o:p></span><td width=128 valign=top style='width:96.0pt;border-top:solid white 1.0pt;
border-left:none;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;
mso-border-left-alt:solid white 1.0pt;background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;
height:29.25pt'>
|- style='mso-yfti-irow:1;height:29.25pt'<td width=136 valign=top style='width:102.0pt;border-top:none;border-left:
solid white 1.0pt;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;
mso-border-top-alt:solid white 3.0pt;background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;
height:29.25pt'><p class=MsoNormal><span style='mso-ansi-language:EN-US'>ICP metal etch SiO2
by reist mask try<o:p></o:p></span><td width=136 valign=top style='width:102.0pt;border-top:none;border-left:
none;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;
mso-border-top-alt:solid white 3.0pt;mso-border-left-alt:solid white 1.0pt;
background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:29.25pt'><p class=MsoNormal><span lang=DA>Date</span><span style='mso-ansi-language:
EN-US'><o:p></o:p></span><td width=108 valign=top style='width:81.0pt;border-top:none;border-left:
none;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;
mso-border-top-alt:solid white 3.0pt;mso-border-left-alt:solid white 1.0pt;
background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:29.25pt'><p class=MsoNormal><span lang=DA>Feb252013</span><span style='mso-ansi-language:
EN-US'><o:p></o:p></span><td width=119 valign=top style='width:89.0pt;border-top:none;border-left:
none;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;
mso-border-top-alt:solid white 3.0pt;mso-border-left-alt:solid white 1.0pt;
background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:29.25pt'><p class=MsoNormal><span lang=DA>Feb252013</span><span style='mso-ansi-language:
EN-US'><o:p></o:p></span><td width=121 valign=top style='width:91.0pt;border-top:none;border-left:
none;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;
mso-border-top-alt:solid white 3.0pt;mso-border-left-alt:solid white 1.0pt;
background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:29.25pt'><p class=MsoNormal><span lang=DA>Feb262013</span><span style='mso-ansi-language:
EN-US'><o:p></o:p></span><td width=128 valign=top style='width:96.0pt;border-top:none;border-left:
none;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;
mso-border-top-alt:solid white 3.0pt;mso-border-left-alt:solid white 1.0pt;
background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:29.25pt'>
|- style='mso-yfti-irow:2;height:29.25pt'<td width=136 valign=top style='width:102.0pt;border-top:none;border-left:
solid white 1.0pt;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;
mso-border-top-alt:solid white 3.0pt;background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;
height:29.25pt'><td width=136 valign=top style='width:102.0pt;border-top:none;border-left:
none;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;
mso-border-top-alt:solid white 3.0pt;mso-border-left-alt:solid white 1.0pt;
background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:29.25pt'><p class=MsoNormal><span lang=DA>Metal <span class=GramE>ICP<span
style='mso-spacerun:yes'>  </span><span class=SpellE>recipe</span></span></span><span
style='mso-ansi-language:EN-US'><o:p></o:p></span><td width=108 valign=top style='width:81.0pt;border-top:none;border-left:
none;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;
mso-border-top-alt:solid white 3.0pt;mso-border-left-alt:solid white 1.0pt;
background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:29.25pt'><p class=MsoNormal><span lang=DA>pxSiO2try3</span><span style='mso-ansi-language:
EN-US'><o:p></o:p></span><td width=119 valign=top style='width:89.0pt;border-top:none;border-left:
none;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;
mso-border-top-alt:solid white 3.0pt;mso-border-left-alt:solid white 1.0pt;
background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:29.25pt'><p class=MsoNormal><span lang=DA>pxSiO2try4</span><span style='mso-ansi-language:
EN-US'><o:p></o:p></span><td width=121 valign=top style='width:91.0pt;border-top:none;border-left:
none;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;
mso-border-top-alt:solid white 3.0pt;mso-border-left-alt:solid white 1.0pt;
background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:29.25pt'><p class=MsoNormal><span lang=DA>pxSiO2try5</span><span style='mso-ansi-language:
EN-US'><o:p></o:p></span><td width=128 valign=top style='width:96.0pt;border-top:none;border-left:
none;border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;
mso-border-top-alt:solid white 3.0pt;mso-border-left-alt:solid white 1.0pt;
background:#4F81BD;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:29.25pt'>
|- style='mso-yfti-irow:3;height:29.25pt'<td width=136 style='width:102.0pt;border-top:none;border-left:solid white 1.0pt;
border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 3.0pt;background:#D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;
height:29.25pt'><td width=136 style='width:102.0pt;border-top:none;border-left:none;
border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 3.0pt;mso-border-left-alt:solid white 1.0pt;background:#D0D8E8;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span class=SpellE><span lang=DA>Wafer</span></span><span
lang=DA><span class=SpellE>size</span> and ID</span><span style='mso-ansi-language:
EN-US'><o:p></o:p></span><td width=108 style='width:81.0pt;border-top:none;border-left:none;
border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 3.0pt;mso-border-left-alt:solid white 1.0pt;background:#D0D8E8;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span lang=DA>6inch,</span><span style='mso-ansi-language:
EN-US'><o:p></o:p></span><p class=MsoNormal><span lang=DA>6A1_feb252013</span><span style='mso-ansi-language:
EN-US'><o:p></o:p></span><td width=119 style='width:89.0pt;border-top:none;border-left:none;
border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 3.0pt;mso-border-left-alt:solid white 1.0pt;background:#D0D8E8;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span lang=DA>6inch,</span><span style='mso-ansi-language:
EN-US'><o:p></o:p></span><p class=MsoNormal><span lang=DA>6A6_feb252013</span><span style='mso-ansi-language:
EN-US'><o:p></o:p></span><td width=121 style='width:91.0pt;border-top:none;border-left:none;
border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 3.0pt;mso-border-left-alt:solid white 1.0pt;background:#D0D8E8;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span lang=DA>6inch,</span><span style='mso-ansi-language:
EN-US'><o:p></o:p></span><p class=MsoNormal><span lang=DA>6A1_feb252013</span><span style='mso-ansi-language:
EN-US'><o:p></o:p></span><td width=128 style='width:96.0pt;border-top:none;border-left:none;
border-bottom:solid white 3.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 3.0pt;mso-border-left-alt:solid white 1.0pt;background:#D0D8E8;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'>
|- style='mso-yfti-irow:4;height:42.9pt'<td width=136 style='width:102.0pt;border:solid white 1.0pt;border-top:none;
mso-border-top-alt:solid white 3.0pt;background:#D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;
height:42.9pt'><td width=136 style='width:102.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 3.0pt;mso-border-left-alt:solid white 1.0pt;background:#D0D8E8;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:42.9pt'><p class=MsoNormal><span lang=DA>Mask</span><span style='mso-ansi-language:
EN-US'><o:p></o:p></span><td width=108 style='width:81.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 3.0pt;mso-border-left-alt:solid white 1.0pt;background:#D0D8E8;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:42.9pt'><p class=MsoNormal><span style='mso-ansi-language:EN-US'>980nm resist resist
on 62nmBarc on 1190nm apox<o:p></o:p></span><td width=119 style='width:89.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 3.0pt;mso-border-left-alt:solid white 1.0pt;background:#D0D8E8;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:42.9pt'><p class=MsoNormal><span style='mso-ansi-language:EN-US'>780nm resist on
62nmBarc on 492nm apox, first etch barc 20sec by Ox plasma<o:p></o:p></span><td width=121 style='width:91.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 3.0pt;mso-border-left-alt:solid white 1.0pt;background:#D0D8E8;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:42.9pt'><p class=MsoNormal><span style='mso-ansi-language:EN-US'>440nm resist on
62nmBarc on 1800nm apox, first etch barc 20sec by Ox plasma<o:p></o:p></span><td width=128 style='width:96.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 3.0pt;mso-border-left-alt:solid white 1.0pt;background:#D0D8E8;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:42.9pt'>
|- style='mso-yfti-irow:5;height:29.25pt'<td width=136 style='width:102.0pt;border:solid white 1.0pt;border-top:none;
mso-border-top-alt:solid white 1.0pt;background:#E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;
height:29.25pt'><td width=136 style='width:102.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#E9EDF4;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span class=SpellE><span lang=DA>Etch</span></span><span
lang=DA> time</span><span style='mso-ansi-language:EN-US'><o:p></o:p></span><td width=108 style='width:81.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#E9EDF4;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span lang=DA>3min</span><span style='mso-ansi-language:
EN-US'><o:p></o:p></span><td width=119 style='width:89.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#E9EDF4;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span lang=DA>3min</span><span style='mso-ansi-language:
EN-US'><o:p></o:p></span><td width=121 style='width:91.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#E9EDF4;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span lang=DA>2min</span><span style='mso-ansi-language:
EN-US'><o:p></o:p></span><td width=128 style='width:96.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#E9EDF4;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'>
|- style='mso-yfti-irow:6;height:29.25pt'<td width=136 style='width:102.0pt;border:solid white 1.0pt;border-top:none;
mso-border-top-alt:solid white 1.0pt;background:#E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;
height:29.25pt'><td width=136 style='width:102.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#E9EDF4;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span lang=DA>Pressure [<span class=SpellE>mTorr</span>] </span><span
style='mso-ansi-language:EN-US'><o:p></o:p></span><td width=108 style='width:81.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#E9EDF4;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span lang=DA>15</span><span style='mso-ansi-language:
EN-US'><o:p></o:p></span><td width=119 style='width:89.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#E9EDF4;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span lang=DA>8</span><span style='mso-ansi-language:EN-US'><o:p></o:p></span><td width=121 style='width:91.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#E9EDF4;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span lang=DA>6</span><span style='mso-ansi-language:EN-US'><o:p></o:p></span><td width=128 style='width:96.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#E9EDF4;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'>
|- style='mso-yfti-irow:7;height:29.25pt'<td width=136 style='width:102.0pt;border:solid white 1.0pt;border-top:none;
mso-border-top-alt:solid white 1.0pt;background:#E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;
height:29.25pt'><td width=136 style='width:102.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#E9EDF4;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span lang=DA>C4F8 flow [<span class=SpellE>sccm</span>] </span><span
style='mso-ansi-language:EN-US'><o:p></o:p></span><td width=108 style='width:81.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#E9EDF4;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span lang=DA>0</span><span style='mso-ansi-language:EN-US'><o:p></o:p></span><td width=119 style='width:89.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#E9EDF4;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span lang=DA>0</span><span style='mso-ansi-language:EN-US'><o:p></o:p></span><td width=121 style='width:91.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#E9EDF4;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span lang=DA>0</span><span style='mso-ansi-language:EN-US'><o:p></o:p></span><td width=128 style='width:96.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#E9EDF4;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'>
|- style='mso-yfti-irow:8;height:29.25pt'<td width=136 style='width:102.0pt;border:solid white 1.0pt;border-top:none;
mso-border-top-alt:solid white 1.0pt;background:#E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;
height:29.25pt'><td width=136 style='width:102.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#E9EDF4;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span lang=DA>CF4 flow [<span class=SpellE>sccm</span>] </span><span
style='mso-ansi-language:EN-US'><o:p></o:p></span><td width=108 style='width:81.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#E9EDF4;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span lang=DA>40</span><span style='mso-ansi-language:
EN-US'><o:p></o:p></span><td width=119 style='width:89.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#E9EDF4;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span lang=DA>40</span><span style='mso-ansi-language:
EN-US'><o:p></o:p></span><td width=121 style='width:91.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#E9EDF4;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span lang=DA>40</span><span style='mso-ansi-language:
EN-US'><o:p></o:p></span><td width=128 style='width:96.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#E9EDF4;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'>
|- style='mso-yfti-irow:9;height:29.25pt'<td width=136 style='width:102.0pt;border:solid white 1.0pt;border-top:none;
mso-border-top-alt:solid white 1.0pt;background:#E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;
height:29.25pt'><td width=136 style='width:102.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#E9EDF4;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span lang=DA>H2 flow [<span class=SpellE>sccm</span>] </span><span
style='mso-ansi-language:EN-US'><o:p></o:p></span><td width=108 style='width:81.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#E9EDF4;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span lang=DA>30</span><span style='mso-ansi-language:
EN-US'><o:p></o:p></span><td width=119 style='width:89.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#E9EDF4;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span lang=DA>30</span><span style='mso-ansi-language:
EN-US'><o:p></o:p></span><td width=121 style='width:91.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#E9EDF4;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span lang=DA>30</span><span style='mso-ansi-language:
EN-US'><o:p></o:p></span><td width=128 style='width:96.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#E9EDF4;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'>
|- style='mso-yfti-irow:10;height:29.25pt'<td width=136 style='width:102.0pt;border:solid white 1.0pt;border-top:none;
mso-border-top-alt:solid white 1.0pt;background:#E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;
height:29.25pt'><td width=136 style='width:102.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#E9EDF4;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span class=SpellE><span lang=DA>Coil</span></span><span
lang=DA> Power [W] </span><span style='mso-ansi-language:EN-US'><o:p></o:p></span><td width=108 style='width:81.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#E9EDF4;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span lang=DA>800</span><span style='mso-ansi-language:
EN-US'><o:p></o:p></span><td width=119 style='width:89.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#E9EDF4;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span lang=DA>800</span><span style='mso-ansi-language:
EN-US'><o:p></o:p></span><td width=121 style='width:91.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#E9EDF4;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span lang=DA>800</span><span style='mso-ansi-language:
EN-US'><o:p></o:p></span><td width=128 style='width:96.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#E9EDF4;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'>
|- style='mso-yfti-irow:11;height:29.25pt'<td width=136 style='width:102.0pt;border:solid white 1.0pt;border-top:none;
mso-border-top-alt:solid white 1.0pt;background:#D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;
height:29.25pt'><td width=136 style='width:102.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#D0D8E8;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span class=SpellE><span lang=DA>Platen</span></span><span
lang=DA> Power [W] </span><span style='mso-ansi-language:EN-US'><o:p></o:p></span><td width=108 style='width:81.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#D0D8E8;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span lang=DA>200 </span><span style='mso-ansi-language:
EN-US'><o:p></o:p></span><td width=119 style='width:89.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#D0D8E8;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span lang=DA>200 </span><span style='mso-ansi-language:
EN-US'><o:p></o:p></span><td width=121 style='width:91.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#D0D8E8;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span lang=DA>100</span><span style='mso-ansi-language:
EN-US'><o:p></o:p></span><td width=128 style='width:96.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#D0D8E8;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'>
|- style='mso-yfti-irow:12;height:29.25pt'<td width=136 style='width:102.0pt;border:solid white 1.0pt;border-top:none;
mso-border-top-alt:solid white 1.0pt;background:#E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;
height:29.25pt'><td width=136 style='width:102.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#E9EDF4;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span class=SpellE><span lang=DA>Platen</span></span><span
lang=DA> temperature [<span class=SpellE><sup>o</sup>C</span>] </span><span
style='mso-ansi-language:EN-US'><o:p></o:p></span><td width=108 style='width:81.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#E9EDF4;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span lang=DA>20 </span><span style='mso-ansi-language:
EN-US'><o:p></o:p></span><td width=119 style='width:89.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#E9EDF4;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span lang=DA>20 </span><span style='mso-ansi-language:
EN-US'><o:p></o:p></span><td width=121 style='width:91.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#E9EDF4;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span lang=DA>20</span><span style='mso-ansi-language:
EN-US'><o:p></o:p></span><td width=128 style='width:96.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#E9EDF4;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'>
|- style='mso-yfti-irow:13;height:29.25pt'<td width=136 style='width:102.0pt;border:solid white 1.0pt;border-top:none;
mso-border-top-alt:solid white 1.0pt;background:#D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;
height:29.25pt'><td width=136 style='width:102.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#D0D8E8;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span class=SpellE><span lang=DA>Coil</span></span><span
lang=DA> match</span><span style='mso-ansi-language:EN-US'><o:p></o:p></span><td width=108 style='width:81.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#D0D8E8;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span class=GramE><span lang=DA>50%</span></span><span
lang=DA>, 30%</span><span style='mso-ansi-language:EN-US'><o:p></o:p></span><td width=119 style='width:89.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#D0D8E8;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span class=GramE><span lang=DA>59%</span></span><span
lang=DA>, 27%</span><span style='mso-ansi-language:EN-US'><o:p></o:p></span><td width=121 style='width:91.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#D0D8E8;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span class=GramE><span lang=DA>60%</span></span><span
lang=DA>,27%</span><span style='mso-ansi-language:EN-US'><o:p></o:p></span><td width=128 style='width:96.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#D0D8E8;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'>
|- style='mso-yfti-irow:14;height:29.25pt'<td width=136 style='width:102.0pt;border:solid white 1.0pt;border-top:none;
mso-border-top-alt:solid white 1.0pt;background:#D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;
height:29.25pt'><td width=136 style='width:102.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#D0D8E8;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span class=SpellE><span lang=DA>Platen</span></span><span
lang=DA> Match</span><span style='mso-ansi-language:EN-US'><o:p></o:p></span><td width=108 style='width:81.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#D0D8E8;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span class=GramE><span lang=DA>50%</span></span><span
lang=DA>, 57%</span><span style='mso-ansi-language:EN-US'><o:p></o:p></span><td width=119 style='width:89.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#D0D8E8;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span class=GramE><span lang=DA>44%</span></span><span
lang=DA>, 56%</span><span style='mso-ansi-language:EN-US'><o:p></o:p></span><td width=121 style='width:91.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#D0D8E8;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span class=GramE><span lang=DA>40%</span></span><span
lang=DA>,53%</span><span style='mso-ansi-language:EN-US'><o:p></o:p></span><td width=128 style='width:96.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#D0D8E8;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'>
|- style='mso-yfti-irow:15;height:29.25pt'<td width=136 style='width:102.0pt;border:solid white 1.0pt;border-top:none;
mso-border-top-alt:solid white 1.0pt;background:#E9EDF4;padding:2.25pt 2.25pt 2.25pt 2.25pt;
height:29.25pt'><td width=136 style='width:102.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#E9EDF4;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span class=SpellE><span lang=DA>Throde</span></span><span
lang=DA><span class=SpellE>valve</span><span class=SpellE>opening</span>
rate</span><span style='mso-ansi-language:EN-US'><o:p></o:p></span><td width=108 style='width:81.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#E9EDF4;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span class=GramE><span lang=DA>10%</span></span><span
style='mso-ansi-language:EN-US'><o:p></o:p></span><td width=119 style='width:89.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#E9EDF4;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span lang=DA>13.<span class=GramE>6%</span></span><span
style='mso-ansi-language:EN-US'><o:p></o:p></span><td width=121 style='width:91.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#E9EDF4;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'><p class=MsoNormal><span class=GramE><span lang=DA>17%</span></span><span
style='mso-ansi-language:EN-US'><o:p></o:p></span><td width=128 style='width:96.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#E9EDF4;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:29.25pt'>
|- style='mso-yfti-irow:16;mso-yfti-lastrow:yes;height:52.5pt'<td width=136 style='width:102.0pt;border:solid white 1.0pt;border-top:none;
mso-border-top-alt:solid white 1.0pt;background:#D0D8E8;padding:2.25pt 2.25pt 2.25pt 2.25pt;
height:52.5pt'><td width=136 style='width:102.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#D0D8E8;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:52.5pt'><p class=MsoNormal><span class=SpellE><span lang=DA>Comments</span></span><span
lang=DA></span><span style='mso-ansi-language:EN-US'><o:p></o:p></span><td width=108 style='width:81.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#D0D8E8;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:52.5pt'><p class=MsoNormal><span class=SpellE><span style='mso-ansi-language:EN-US'>Apox</span></span><span
style='mso-ansi-language:EN-US'> etch 550nm for 3min, side wall angle
71degree<o:p></o:p></span><td width=119 style='width:89.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#D0D8E8;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:52.5pt'><p class=MsoNormal><span style='mso-ansi-language:EN-US'>Too much polymer,
etch Si too much<o:p></o:p></span><p class=MsoNormal><span style='mso-ansi-language:EN-US'>Etch through 500nm <span
class=SpellE>apox</span>, then etch Si 180nm,<o:p></o:p></span><td width=121 style='width:91.0pt;border-top:none;border-left:none;
border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;mso-border-top-alt:
solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;background:#D0D8E8;
padding:2.25pt 2.25pt 2.25pt 2.25pt;height:52.5pt'><p class=MsoNormal><span style='mso-ansi-language:EN-US'>Profile Very good,
2min etch SiO3 350nm in wafer center, 310nm in wafer, resist etched 260nm<o:p></o:p></span><td width=128 valign=top style='width:96.0pt;border-top:none;border-left:
none;border-bottom:solid white 1.0pt;border-right:solid white 1.0pt;
mso-border-top-alt:solid white 1.0pt;mso-border-left-alt:solid white 1.0pt;
background:#D0D8E8;padding:3.6pt 7.2pt 3.6pt 7.2pt;height:52.5pt'><p class=MsoNormal><span style='mso-ansi-language:EN-US'>Low pressure gives
better profile, less polymer, however, CF4 etch Si too quick<o:p></o:p></span>
|}<p class=MsoNormal><span style='mso-ansi-language:EN-US'><o:p> </o:p></span></div></body></html>

Latest revision as of 09:31, 10 February 2023

Feedback to this page: click here
This page is written by Berit Herstrøm @ DTU Nanolab (BGHE) if nothing else is stated

With C4F8 and H2 chemistry (all tests done by Peixiong Shi, DTU Nanolab)

Part 1

Very good

Very good

Very good

Very good

Very good

Very good

Unstable plasma at 2mtorr

stable plasma at 2.5mtorr

stable plasma at 2.5mtorr

ICP metal etch SiO2 by reist mask try

Date

Feb262013

Feb272013

Feb272013 20:00

Feb272013 23:00

Feb282013 1am

Feb282013 2am

Feb282013 2am

Feb282013 2am

Feb2820134am

Metal ICP  recipe

pxSiO2try5

pxSiO2try6

pxSiO2try7

pxSiO2try8

pxSiO2try8

pxSiO2try8

pxSiO2try9

pxSiO2try9

pxSiO2try9

Wafer size and ID

6inch,

6A1_feb252013

6inch,

6A4_feb262013

6inch,

6A6_feb262013

6inch,

6A2_feb272013

6inch,

6A3_feb272013

6inch,

6A4_feb272013

6inch,

6A5_feb272013

6inch,

6A5_feb272013

6inch,

6A6_feb272013

Mask

440nm resist on 62nmBarc on 1800nm apox, first etch barc 20sec by Ox plasma

440nm resist on 62nmBarc on 1800nm apox, first etch barc 20sec by Ox plasma

780nm resist on 62nmBarc on 1800nm apox, first etch barc 20sec by Ox plasma

780nm resist on 62nmBarc on 800nm apox, first etch barc 20sec by Ox plasma

780nm resist on 62nmBarc on 490nm apox, first etch barc 20sec by Ox plasma

Blank Si

780nm resist on 62nmBarc on 490nm apox, first etch barc 20sec by Ox plasma

780nm resist on 62nmBarc on 490nm apox, first etch barc 20sec by Ox plasma

780nm resist on 62nmBarc on 490nm apox, first etch barc 20sec by Ox plasma

Etch time

2min

4min

4min

4min

5min

4min

1min

4min

5min

Pressure [mTorr]

6

6

4

3

3

2

2

2.5

2.5

C4F8 flow [sccm]

0

20

10

8

8

8

8

8

8

CF4 flow [sccm]

40

0

0

0

0

0

0

0

0

H2 flow [sccm]

30

20

30

30

30

30

30

30

30

CH4 flow [sccm]

0

Set 20 real 3.7

Set 20 real 3.7

0

0

0

0

0

0

Coil Power [W]

800

800

800

800

800

800

800

800 reflect 13W

800 reflect 8W

Platen Power [W]

100

100

120

150

150

150

150

150

150reflect 0.2w

Platen temperature [oC]

20

20

20

20

20

20

20

20

20

Coil match

60%,27%

63%,25%

63%,25%

67%,24%

67%,24%

68.9%,24.1%

68.9%,24.1%

68.7%,25.3%

68.87%,23.1%

Platen Match

40%,53%

36%,54%

36%,54%

34%,54%

34%,54%

34.3%,53.8%

34.3%,53.8%

36.8%,54.9%

33.0%,54.4%

Throde valve opening rate

17%

12%

14%

14.7%

14.7%

14.7%

14.7%

16.2%

Images

Image1

Images

Images3

Images4

Iamges5

Images6

Images7

Images

Comments

Profile Very good, 2min etch SiO3 350nm in wafer center, 310nm in wafer, resist etched 260nm

Profile Very good, 2min etch SiO3 350nm in wafer center, 310nm in wafer, resist etched 260nm

Profile Very good, 4min etch SiO3 480nm in wafer center, Resist etched 100nm

Profile Very good, 4min etch SiO3 480nm in wafer center, Resist etched 100nm, side wall 85degree

Profile Very good, 4min etch SiO3 480nm in wafer center, Resist etched 100nm

Plasma very stable on blank Si wafer

Plasma not stable in apox wafer

etched 500nm apox, resit 150n, slide wall  86degm

 

Part2

ICP metal etch SiO2 by reist mask try

stable plasma at 2.5mtorr

stable plasma at 2.5mtorr

Date

Feb28204am

March012013, 21

Metal ICP  recipe

pxSiO2try9

pxSiO2try9

Wafer size and ID

6inch,

6A6_feb272013

6inch,

6A1_march012013

Mask

780nm resist on 62nmBarc on 490nm apox, first etch barc 20sec by Ox plasma

780nm resist on 62nmBarc on 490nm apox, first etch barc 20sec by Ox plasma

Etch time

5min

65min

Pressure [mTorr]

2.5

2.5

C4F8 flow [sccm]

8

8

CF4 flow [sccm]

0

0

H2 flow [sccm]

30

30

CH4 flow [sccm]

0

0

Coil Power [W]

800 reflect 8W

800 reflect 8W

Platen Power [W]

150reflect 0.2w

150reflect 0.2w

Platen temperature [oC]

20

20

Coil match

68.87%,23.1%

68.87%,23.1%

Platen Match

33.0%,54.4%

33.0%,54.4%

Throde valve opening rate

10.8% to 11.7%, pressure 2.11 to 2.40, not stable

Comments

SiO2 width 230nm

 

With CF4 and H2 chemistry by Peixiong Shi, DTU Nanolab

Part 1

bad

bad

bad

bad

bad

Date

Feb122013

Feb122013

Feb122013

Feb122013

Feb122013

Metal ICP  recipe

pxSiO2try1

pxSiO2try1

pxSiO2try1

pxSiO2try2

pxSiO2try2

Wafer size and ID

6inch

6A

6inch

6A1_feb112013

6inch,

6A2_feb112013

6inch,

6A3_feb112013

6inch,

6A4_feb112013

Mask

Blank Si dummy test

Blank apox, 3539nm

Blank KRF 347.9nm

Blank KRF 345nm

Blank  apox 4623m

Etch time

2min

2min

1min

1min

1min

Pressure [mTorr]

8

8

8

20

20

C4F8 flow [sccm]

20

20

20

20

CF4 flow [sccm]

40

40

40

40

40

H2 flow [sccm]

20

20

20

20

20

Coil Power [W]

800

800

800

800

800

Platen Power [W]

200

200

200

200

200

Platen temperature [oC]

20

20

20

20

20

Coil match

59%, 27%

59%, 27%

59%, 27%

48%, 29%

48%, 29%

Platen Match

45%, 56%

45%, 56%

45%, 56%

52%, 60%

52%, 60%

Throde valve opening rate

16%

16%

16%

10.7%

10.7%

Etch rate

µm/min

Wf center  238µm/min

Wafer  edge  230nm/min

Wafer center 170.5nm/min

1cm from wf edge , 204.1nm/min

Wf center  80.4µm/min

Wafer  edge  119.6nm/min

Wafer center 128.26nm/min, 1cm from wafer  edge 123.09nm/min

Distance from wf cent (mm)

Seletivity at cent

Remaining APOX thickness nm

Wf center 3062nm

1cm from wf edge: 3079nm

Wf center nm

Too much polymer in sem

Comments

 

Part 2

bad

bad

bad

Very good

ICP metal etch SiO2 by reist mask try

Date

Feb252013

Feb252013

Feb262013

Metal ICP  recipe

pxSiO2try3

pxSiO2try4

pxSiO2try5

Wafer size and ID

6inch,

6A1_feb252013

6inch,

6A6_feb252013

6inch,

6A1_feb252013

Mask

980nm resist resist on 62nmBarc on 1190nm apox

780nm resist on 62nmBarc on 492nm apox, first etch barc 20sec by Ox plasma

440nm resist on 62nmBarc on 1800nm apox, first etch barc 20sec by Ox plasma

Etch time

3min

3min

2min

Pressure [mTorr]

15

8

6

C4F8 flow [sccm]

0

0

0

CF4 flow [sccm]

40

40

40

H2 flow [sccm]

30

30

30

Coil Power [W]

800

800

800

Platen Power [W]

200

200

100

Platen temperature [oC]

20

20

20

Coil match

50%, 30%

59%, 27%

60%,27%

Platen Match

50%, 57%

44%, 56%

40%,53%

Throde valve opening rate

10%

13.6%

17%

Images

Images 2

Images

Comments

Apox etch 550nm for 3min, side wall angle 71degree

Too much polymer, etch Si too much

Etch through 500nm apox, then etch Si 180nm,

Profile Very good, 2min etch SiO3 350nm in wafer center, 310nm in wafer, resist etched 260nm

Low pressure gives better profile, less polymer, however, CF4 etch Si too quick