| [[Image:UVLithography.jpg|320x320px|right|frame|]] | | '''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Lithography/UVLithography click here]''' |
|
| |
|
| UV Lithography uses ultraviolet light to transfer a pattern from a mask to a wafer coated with photoresist. The photoresist film is spin coated on the wafers and the pattern is transferred to the wafer by using a mask aligner. DTU Danchip houses a number of automatic or semi-automatic coaters and mask aligners.
| | [[Category: Equipment|Lithography]] |
| | [[Category: Lithography]] |
|
| |
|
| = Getting started =
| | [[Image:UVLithography.jpg|400px|right|]] |
|
| |
|
| [[File:UVLPic1.png|450px|right]]
| | __TOC__ |
|
| |
|
| [[File:UVLPic2.png|160px|right]]
| | =UV lithography= |
| | UV Lithography uses ultraviolet light to transfer a pattern from a photo-mask, or a digital design file, to a substrate coated with photoresist. |
|
| |
|
| '''Before you plan your UV processing and request for training on any equipment in UV lithography, please go through the following steps.''' Include the information in the training request.
| | The process has 3 main steps: |
| | # Coating the substrate with a photosensitive film |
| | # Transferring a pattern into the resist by exposing it with UV light through either a physical shadow mask or a digital version of a shadow mask |
| | # Developing the exposed resist to reveal the transferred pattern |
|
| |
|
| If you are new to photolithography, you can visit <u>[https://en.wikipedia.org/wiki/Photolithography this]</u> wikipedia webpage about photolithography before you start.
| | DTU Nanolab offers a number of automatic and manual coaters, mask or maskless exposure tools, as well as automatic or semi-automatic developers.<br clear=all /> |
| <br> <br>
| |
|
| |
|
| * '''Prepare a process flow''' which describes all steps in your UV lithography process. You can find docx-templates <u>[[Specific_Process_Knowledge/Lithography/UVLithography#Resist_Overview|in this table]]</u>.
| | =Getting started with UV lithography= |
|
| |
|
| * '''Substrate pretreatment''': In many processes it is recommended to <u>[[Specific_Process_Knowledge/Lithography/Pretreatment|pretreat or prime]]</u> your wafer before spin-coating. In some <u>[[Specific_Process_Knowledge/Lithography/Coaters|spin-coaters]]</u>, these pretreatment processes are included in the spin coating of resist.
| | [[File:UVLPic1.png|450px|right]] |
|
| |
|
| * '''Spin Coater''': Do you wish to use a manual spin coater or a robot spin coater? See a list of spin coaters <u>[[Specific_Process_Knowledge/Lithography/Coaters|here]]</u>.
| | [[File:UVLPic2.png|160px|right]] |
|
| |
|
| * '''Resist Type''': Choose the type of resist you wish to use: a list of UV lithography resist types available at DTU Danchip can be found <u>[[Specific_Process_Knowledge/Lithography/UVLithography#Resist_Overview|on this page]]</u>.
| | <span style="color:red">New users are always recommended to have their process evaluated by the fabrication support group - before you start planning your UV process, and request training on UV lithography equipment, please go through the following pre-cleanroom and cleanroom steps and include all the information in your request.</span> |
| ** Positive tone resist: Resist exposed to UV light will be dissolved in the developer. The mask openings are an exact copy of the resist pattern which is to remain on the wafer.
| |
| ** Negative tone resist: Resist exposed to UV light will become polymerized and difficult to dissolve. The mask openings are an inverse copy of the resist pattern which is to remain on the wafer.
| |
|
| |
|
| * '''Thickness of resist''': In general, it is recommended to work at or below an aspect ratio of ~1, i.e. where the width of the pattern is larger than the thickness of the resist. Furthermore, when you decide for the resist thickness, consider which transfer you need:
| | Please remember that the [https://labadviser.nanolab.dtu.dk//index.php?title=Specific_Process_Knowledge/Lithography#Lithography_Tool_Package_Training Lithography TPT] is <i>mandatory</i> before you can receive training on any lithography equipment.<br> |
| ** For <u>[[Specific_Process_Knowledge/Lithography/LiftOff|lift-off]]</u> processes, we recommend resist thickness at least 5 times larger than the thickness of the metal to be lifted.
| | If you are completely new to photolithography, you can visit <u>[https://en.wikipedia.org/wiki/Photolithography this]</u> wikipedia webpage about photolithography before you start. |
| ** For dry etch or wet etch processes, investigate the resist etch rate of your process as this might limit the minimum thickness of your resist.
| |
|
| |
|
| *'''Exposure''': Choose which mask aligner you wish to use, and consider the exposure dose.
| |
| ** You can find a list of mask aligners <u>[[Specific_Process_Knowledge/Lithography/UVExposure|here]]</u>.
| |
| ** You can find information on dose <u>[[Specific_Process_Knowledge/Lithography/UVExposure_Dose|here]]</u>.
| |
|
| |
|
| * '''Mask''': Design and order a photomask for your UV process. A detailed instruction on how to design and order a photomask can be found <u>[[Specific_Process_Knowledge/Lithography/Pattern_Design_and_Mask_Fabrication|here]]</u>.
| | '''Pre-cleanroom work:''' |
| | # Complete the [https://labadviser.nanolab.dtu.dk//index.php?title=Specific_Process_Knowledge/Lithography#Lithography_Tool_Package_Training Lithography TPT] |
| | # Prepare a process flow: The process flow describes all steps in your UV lithography process. You can find docx-templates <u>[[Specific_Process_Knowledge/Lithography/Resist/UVresist#UV_resist_comparison_table|in this table]]</u> |
| | # Evaluate your process in cooperation with the fabrication support group |
| | # Design device: Design your device and layout. A detailed instruction on how to design a layout (or mask) can be found <u>[[Specific_Process_Knowledge/Pattern_Design|here]]</u> |
| | # Mask: If you wish to use a mask aligner, order a photomask for your UV process. Instructions on how to order a photomask can be found <u>[[Specific_Process_Knowledge/Pattern_Design#Mask_Ordering_and_Fabrication|here]]</u> |
|
| |
|
| * '''Development''': Choose which equipment you wish to use to develop your photoresist from <u>[[Specific_Process_Knowledge/Lithography/Development|this list]]</u>. Remember the development chemistry influences the <u>[[Specific_Process_Knowledge/Lithography/UVExposure_Dose|exposure dose]]</u>.
| |
|
| |
|
| * '''Specify whether you wish to strip or lift-off your resist''': <u>[[Specific_Process_Knowledge/Lithography/Strip|strip]]</u> and <u>[[Specific_Process_Knowledge/Lithography/LiftOff|lift-off]]</u>. | | '''Cleanroom work:''' |
| | # Substrate pretreatment: In many processes it is recommended to <u>[[Specific_Process_Knowledge/Lithography/Pretreatment|pre-treat or prime]]</u> your wafer before coating. In some <u>[[Specific_Process_Knowledge/Lithography/Coaters|spin coaters]]</u>, these pre-treatment processes are included in the spin coating of resist |
| | # Resist Type: Choose the type of resist you wish to use: a list of UV lithography resist types available at DTU Nanolab can be found <u>[[Specific_Process_Knowledge/Lithography/Resist#UV_Resist|on this page]]</u> |
| | #*Positive tone resist: Resist exposed to UV light will be dissolved in the developer. For mask aligners, the mask openings are an exact copy of the resist pattern which is to remain on the wafer |
| | #*Negative tone resist: Resist exposed to UV light will become polymerized and difficult to dissolve. For mask aligners, the mask openings are an ''inverse'' copy of the resist pattern which is to remain on the wafer |
| | # Thickness of resist: In general, it is recommended to work at, or below, an aspect ratio of ~1, i.e. where the feature sizes of the pattern, is larger than the thickness of the resist. Furthermore, when you decide on the resist thickness, consider which transfer method you need: |
| | #*For <u>[[Specific_Process_Knowledge/Lithography/LiftOff|lift-off]]</u> processes, we recommend resist thickness at least 5 times larger than the thickness of the metal to be lifted |
| | #*For dry etch or wet etch processes, investigate the resist etch rate of your process, as this might limit the ''minimum'' thickness of your resist |
| | # Spin Coater: Do you need to use a manual spin coater or an automatic spin coater? See a list of spin coaters <u>[[Specific_Process_Knowledge/Lithography/Coaters|here]]</u> |
| | # Exposure: Choose which aligner you wish to use, and consider the exposure dose |
| | #*You can find a list of mask aligners and maskless aligners <u>[[Specific_Process_Knowledge/Lithography/UVExposure|here]]</u> |
| | #*You can find information on dose <u>[[Specific_Process_Knowledge/Lithography/Resist#UV_Resist|here]]</u> |
| | # Development: Choose which equipment you wish to use to develop your photoresist from <u>[[Specific_Process_Knowledge/Lithography/Development|this list]]</u>. Remember the development process influences the <u>[[Specific_Process_Knowledge/Lithography/Resist#UV_Resist|exposure dose]]</u> |
| | # Specify whether you wish to strip or lift-off your resist: <u>[[Specific_Process_Knowledge/Lithography/Strip|strip]]</u> and <u>[[Specific_Process_Knowledge/Lithography/LiftOff|lift-off]]</u> |
|
| |
|
| <br clear=all />
| |
|
| |
|
| = Resist Overview = | | ==Mask Aligner versus Maskless Aligner== |
|
| |
|
| {|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" width="90%"
| | [[Specific_Process_Knowledge/Lithography/Aligners/MAvsMLA|Mask Aligner vs Maskless Aligner]] |
| |-
| |
|
| |
|
| |-
| | <br clear=all /> |
| |-style="background:silver; color:black"
| |
| |'''Resist'''
| |
| |width=100|'''Polarity'''
| |
| |'''Spectral sensitivity'''
| |
| |'''Manufacturer'''
| |
| |width=200|'''Comments'''
| |
| |width=100|'''Technical reports'''
| |
| |'''[[Specific_Process_Knowledge/Lithography/Coaters|Spin Coating]]'''
| |
| |'''[[Specific_Process_Knowledge/Lithography/UVExposure|Exposure]]'''
| |
| |'''[[Specific_Process_Knowledge/Lithography/Development|Developer]]'''
| |
| |'''Rinse'''
| |
| |width=100|'''Remover'''
| |
| |'''Process flows (in docx-format)'''
| |
| | |
| |-
| |
| | |
| |-
| |
| |-style="background:WhiteSmoke; color:black"
| |
| |'''AZ 5214E'''
| |
| |Positive but the image can be reversed
| |
| |310 - 420 nm
| |
| |[http://www.azem.com/en/Products/Litho-technology/Photoresists.aspx AZ Electronic Materials]
| |
| |Can be used for both positive and reverse processes with resist thickness between 1 and 4 µm.
| |
| |[[media:AZ5214E.pdf|AZ5214E.pdf]]
| |
| |[[Specific_Process_Knowledge/Lithography/Coaters#Spin_Coater:_Gamma_UV|Spin Coater: Gamma UV]],
| |
| | |
| [[Specific_Process_Knowledge/Lithography/Coaters#Manual_Spin_Coaters|A manual spin coater]] or
| |
| | |
| [[Specific_Process_Knowledge/Lithography/Coaters#Spin_Coater:_RCD8|Spin Coater: RCD8]]
| |
| |[[Specific_Process_Knowledge/Lithography/UVExposure#KS_Aligner|KS Aligner]],
| |
| | |
| [[Specific_Process_Knowledge/Lithography/UVExposure#Aligner:_MA6_-_2|Aligner: MA6 - 2]] or
| |
| | |
| [[Specific_Process_Knowledge/Lithography/UVExposure#Aligner-6inch|Aligner: 6inch]]
| |
| |[[Specific_Process_Knowledge/Lithography/Development#Developer-6inch|AZ 351B developer]]
| |
| | |
| or
| |
| | |
| [[Specific_Process_Knowledge/Lithography/Development#Developer_TMAH_UV-lithography|AZ 726 MIF developer]]
| |
| |DI water
| |
| |Acetone
| |
| |
| |
| [[media:Process_Flow_AZ5214E_pos_vers2.docx |Process_Flow_AZ5214_pos.docx]]
| |
| [[media:Process_Flow_AZ5214E_rev_vers2.docx |Process_Flow_AZ5214_rev.docx]]
| |
| | |
| |-
| |
| |-style="background:LightGrey; color:black"
| |
| |'''AZ 4562'''
| |
| |Positive
| |
| |310 - 440 nm
| |
| |[http://www.azem.com/en/Products/Litho-technology/Photoresists.aspx AZ Electronic Materials]
| |
| |For process with resist thickness between 6 and 25 µm.
| |
| |[[media:AZ4500.pdf|AZ4500.pdf]]
| |
| |[[Specific_Process_Knowledge/Lithography/Coaters#SSE Spinner|SSE]],
| |
| | |
| [[Specific_Process_Knowledge/Lithography/Coaters#Manual_Spin_Coaters|A manual spin coater]] or
| |
| | |
| [[Specific_Process_Knowledge/Lithography/Coaters#Spin_Coater:_RCD8|Spin Coater: RCD8]]
| |
| |[[Specific_Process_Knowledge/Lithography/UVExposure#KS_Aligner|KS Aligner]],
| |
| | |
| [[Specific_Process_Knowledge/Lithography/UVExposure#Aligner:_MA6_-_2|Aligner: MA6 - 2]] or
| |
| | |
| [[Specific_Process_Knowledge/Lithography/UVExposure#Aligner-6inch|Aligner: 6inch]]
| |
| |[[Specific_Process_Knowledge/Lithography/Development#Developer-6inch|AZ 351B developer]]
| |
| | |
| or
| |
| | |
| [[Specific_Process_Knowledge/Lithography/Development#Developer_TMAH_UV-lithography|AZ 726 MIF developer]]
| |
| |DI water
| |
| |Acetone
| |
| |[[media:Process_Flow_thick_AZ4562_vers2.docx|Process_Flow_thick_AZ4562.docx]]
| |
| | |
| |-
| |
| |-style="background:WhiteSmoke; color:black"
| |
| |'''AZ MiR 701'''
| |
| |Positive
| |
| |310 - 445 nm
| |
| |[http://www.azem.com/en/Products/Litho-technology/Photoresists.aspx AZ Electronic Materials]
| |
| |High selectivity for dry etch.
| |
| | |
| Resist thickness 1 - 2 µm.
| |
| |[[media:AZ_MiR_701.pdf|AZ_MiR_701.pdf]]
| |
| |[[Specific_Process_Knowledge/Lithography/Coaters#Spin_Coater:_Gamma_UV|Spin Coater: Gamma UV]],
| |
| | |
| [[Specific_Process_Knowledge/Lithography/Coaters#Spin Track 1 + 2|Spin Track 1 + 2]],
| |
| | |
| [[Specific_Process_Knowledge/Lithography/Coaters#Manual_Spin_Coaters|A manual spin coater]] or
| |
| | |
| [[Specific_Process_Knowledge/Lithography/Coaters#Spin_Coater:_RCD8|Spin Coater: RCD8]]
| |
| |[[Specific_Process_Knowledge/Lithography/UVExposure#KS_Aligner|KS Aligner]],
| |
| | |
| [[Specific_Process_Knowledge/Lithography/UVExposure#Aligner:_MA6_-_2|Aligner: MA6 - 2]] or
| |
| | |
| [[Specific_Process_Knowledge/Lithography/UVExposure#Aligner-6inch|Aligner: 6inch]]
| |
| |[[Specific_Process_Knowledge/Lithography/Development#Developer_TMAH_UV-lithography|AZ 726 MIF developer]]
| |
| |DI water
| |
| |Remover 1165
| |
| |[[media:Process_Flow_AZ_MiR701.docx|Process_Flow_AZ_MiR701.docx]]
| |
| | |
| |-
| |
| |-style="background:LightGrey; color:black"
| |
| |'''AZ nLOF 2020'''
| |
| |Negative
| |
| |310 - 380 nm
| |
| |[http://www.azem.com/en/Products/Litho-technology/Photoresists.aspx AZ Electronic Materials]
| |
| |Negative sidewalls for lift-off.
| |
| | |
| Resist thickness 1.5 - 3 µm.
| |
| |[[media:AZ_nLOF_2020.pdf|AZ_nLOF_2020.pdf]]
| |
| |[[Specific_Process_Knowledge/Lithography/Coaters#Spin_Coater:_Gamma_UV|Spin Coater: Gamma UV]];
| |
| | |
| [[Specific_Process_Knowledge/Lithography/Coaters#Spin Track 1 + 2|Spin Track 1 + 2]],
| |
| | |
| [[Specific_Process_Knowledge/Lithography/Coaters#Manual_Spin_Coaters|A manual spin coater]] or
| |
| | |
| [[Specific_Process_Knowledge/Lithography/Coaters#Spin_Coater:_RCD8|Spin Coater: RCD8]]
| |
| |[[Specific_Process_Knowledge/Lithography/UVExposure#KS_Aligner|KS Aligner]],
| |
| | |
| [[Specific_Process_Knowledge/Lithography/UVExposure#Aligner:_MA6_-_2|Aligner: MA6 - 2]] or
| |
| | |
| [[Specific_Process_Knowledge/Lithography/UVExposure#Aligner-6inch|Aligner: 6inch]]
| |
| |[[Specific_Process_Knowledge/Lithography/Development#Developer_TMAH_UV-lithography|AZ 726 MIF developer]]
| |
| |DI water
| |
| |Remover 1165
| |
| |[[media:Process_Flow_AZ_nLOF_2020.docx|Process_Flow_AZ_nLOF_2020.docx]]
| |
| | |
| |-
| |
| |-style="background:WhiteSmoke; color:black"
| |
| |'''[[Specific Process Knowledge/Lithography/SU-8|SU-8]]'''
| |
| |Negative
| |
| |350 - 400 nm
| |
| |[http://microchem.com/Prod-SU82000.htm Microchem]
| |
| |High aspect ratio.
| |
| | |
| Resist thickness 1 µm to several 100 µm.
| |
| |[[media:SU-8_DataSheet_2005.pdf|SU-8_DataSheet_2005.pdf]], [[media:SU-8_DataSheet_2075.pdf|SU-8_DataSheet_2075.pdf]]
| |
| |[[Specific_Process_Knowledge/Lithography/Coaters|???]]
| |
| |[[Specific_Process_Knowledge/Lithography/UVExposure#Aligner-6inch|Aligner: 6inch]],
| |
|
| |
|
| [[Specific_Process_Knowledge/Lithography/UVExposure#KS_Aligner|KS Aligner]] or
| | <!--- |
| | =Equipment and Process Pages= |
| | {{:Specific Process Knowledge/Lithography/UVlithographyProcessPages}} |
|
| |
|
| [[Specific_Process_Knowledge/Lithography/UVExposure#Aligner:_MA6_-_2|Aligner: MA6 - 2]] | | ===[[Specific Process Knowledge/Lithography/Resist#UV_Resist|UV Resist]]=== |
| |[[Specific_Process_Knowledge/Lithography/Development#SU8-Developer|mr-Dev 600 developer (PGMEA)]]
| |
| |IPA
| |
| |Plasma ashing can remove crosslinked SU-8
| |
| |[[media:Process_Flow_SU8_70um.docx|Process_Flow_SU8_70um.docx]]
| |
| | |
| |}
| |
| | |
| <br clear="all" />
| |
| | |
| =Process information= | |
| ===[[Specific Process Knowledge/Lithography/Pretreatment|Pretreatment]]=== | | ===[[Specific Process Knowledge/Lithography/Pretreatment|Pretreatment]]=== |
| ===[[Specific Process Knowledge/Lithography/Coaters|Coaters]]=== | | ===[[Specific Process Knowledge/Lithography/Coaters|Coating]]=== |
| ===[[Specific Process Knowledge/Lithography/UVExposure|UV Exposure]]===
| |
| ===[[Specific_Process_Knowledge/Lithography/UVExposure_Dose|Information on UV Exposure Dose]]===
| |
| ===[[Specific Process Knowledge/Lithography/Baking|Baking]]=== | | ===[[Specific Process Knowledge/Lithography/Baking|Baking]]=== |
| | ===[[Specific Process Knowledge/Lithography/UVExposure|UV Exposure Tools]]=== |
| ===[[Specific Process Knowledge/Lithography/Development|Development]]=== | | ===[[Specific Process Knowledge/Lithography/Development|Development]]=== |
| | ===[[Specific Process Knowledge/Lithography/Descum|Descum]]=== |
| | ===[[Specific Process Knowledge/Lithography/LiftOff|Lift-off]]=== |
| ===[[Specific Process Knowledge/Lithography/Strip|Stripping Resist]]=== | | ===[[Specific Process Knowledge/Lithography/Strip|Stripping Resist]]=== |
| ===[[Specific Process Knowledge/Lithography/LiftOff|Lift-off]]=== | | ---> |
| | |
| | =Process information from our suppliers= |
| | MicroChemicals GmbH has a [https://www.microchemicals.com/downloads/application_notes.html very large online library] of information about UV lithography. |
| | |
| | Of particular interest is the [https://www.microchemicals.com/dokumente/application_notes/lithography_trouble_shooting.pdf lithography trouble-shooter] |