Jump to content

Specific Process Knowledge/Pattern Design/Travka/fields/Tridge: Difference between revisions

From LabAdviser
Jmli (talk | contribs)
Created page with "== The T-ridge field == <!-- revised 1/6-2015 by jmli --> The T-ridge fields contain a triple ridge structure for a number of different ridge widths. The triple ridge structur..."
 
Jmli (talk | contribs)
No edit summary
 
(3 intermediate revisions by the same user not shown)
Line 1: Line 1:
'''Feedback to this page:
[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Pattern/Travka/fields/Tridge click here]'''
<!--Checked for updates on 30/7-2018 - ok/jmli -->
<!--Checked for updates on 5/10-2020 - ok/jmli -->
<!--Checked for updates on 28/6-2023 - ok/jmli -->
<!--Checked for updates on 4/9-2025 - ok/jmli -->
{{Contentbydryetch}}
== The T-ridge field ==
== The T-ridge field ==
<!-- revised 1/6-2015 by jmli -->
<!--Checked for updates on 30/7-2018 - ok/jmli -->
The T-ridge fields contain a triple ridge structure for a number of different ridge widths. The triple ridge structure is shown in the image. [[Image:T-ridge2.jpg |500x500px|thumb|Definition of the measures used in the table below]] It consists of three ridges of a certain width. The two trenches between them have the same width. The three ridges are separated by an etched area that is five times the ridge width. This parameters of this feature is not changed in the different Travka masks. In order to vary the exposed area on each Travka mask a masked area (in the figure called 'space') is added between every feature.
The T-ridge fields contain a triple ridge structure for a number of different ridge widths. The triple ridge structure is shown in the image. [[Image:T-ridge2.jpg |500x500px|thumb|Definition of the measures used in the table below]] It consists of three ridges of a certain width. The two trenches between them have the same width. The three ridges are separated by an etched area that is five times the ridge width. This parameters of this feature is not changed in the different Travka masks. In order to vary the exposed area on each Travka mask a masked area (in the figure called 'space') is added between every feature.



Latest revision as of 10:38, 4 September 2025

Feedback to this page: click here Unless otherwise stated, the content of this page was created by the dry etch group at DTU Nanolab


The T-ridge field

The T-ridge fields contain a triple ridge structure for a number of different ridge widths. The triple ridge structure is shown in the image.

Definition of the measures used in the table below

It consists of three ridges of a certain width. The two trenches between them have the same width. The three ridges are separated by an etched area that is five times the ridge width. This parameters of this feature is not changed in the different Travka masks. In order to vary the exposed area on each Travka mask a masked area (in the figure called 'space') is added between every feature.

Travka 05 T-ridge field

Travka 05: T-ridge 2 µm to 6 µm features
Width (µm) Triple width (µm) Area (µm) Space (µm) Total feature width (µm) Number of features Total width (µm)
2 10 10 450 480 2 960
3 15 15 675 720 1 1680
4 20 20 900 960 1 2640
5 25 25 1125 1200 1 3840
6 30 30 1350 1440 1 5280
Travka 05: T-ridge 8 µm to 20 µm features
Width (µm) Triple width (µm) Area (µm) Space (µm) Total feature width (µm) Number of features Total width (µm)
8 40 40 1800 1920 1 7200
10 50 50 2250 2400 1 9600
15 75 75 3375 3600 1 13200
20 100 100 4500 4800 1 18000


Travka 10 T-ridge field

Travka 10: T-ridge 2 µm to 6 µm features
Width (µm) Triple width (µm) Area (µm) Space (µm) Total feature width (µm) Number of features Total width (µm)
2 10 10 210,0 240 3 720
3 15 15 315,0 360 3 1800
4 20 20 420,0 480 3 3240
5 25 25 525,0 600 3 5040
6 30 30 630,0 720 3 7200
Travka 10: T-ridge 8 µm to 20 µm features
Width (µm) Triple width (µm) Area (µm) Space (µm) Total feature width (µm) Number of features Total width (µm)
8 40 40 840,0 960 2 9120
10 50 50 1050,0 1200 2 11520
15 75 75 1575,0 1800 2 15120
20 100 100 2100,0 2400 2 19920

Travka 20 T-ridge field

Travka 20: T-ridge 2 µm to 6 µm features
Width (µm) Triple width (µm) Area (µm) Space (µm) Total feature width (µm) Number of features Total width (µm)
2 10 10 90,0 120 5 600
3 15 15 135,0 180 6 1680
4 20 20 180,0 240 5 2880
5 25 25 225,0 300 5 4380
6 30 30 270,0 360 5 6180
Travka 20: T-ridge 8 µm to 20 µm features
Width (µm) Triple width (µm) Area (µm) Space (µm) Total feature width (µm) Number of features Total width (µm)
8 40 40 360,0 480 5 8580
10 50 50 450,0 600 5 11580
15 75 75 675,0 900 4 15180
20 100 100 900,0 1200 4 19980


Travka 35 T-ridge field

Travka 35: T-ridge 2 µm to 6 µm features
Width (µm) Triple width (µm) Area (µm) Space (µm) Total feature width (µm) Number of features Total width (µm)
2 10 10 38,6 68,5 7 480
3 15 15 57,9 102,9 7 1200
4 20 20 77,1 137,1 9 2434
5 25 25 96,4 171,4 8 3805
6 30 30 115,7 205,7 8 5451
Travka 35: T-ridge 8 µm to 20 µm features
Width (µm) Triple width (µm) Area (µm) Space (µm) Total feature width (µm) Number of features Total width (µm)
8 40 40 154,3 274,3 8 7646
10 50 50 192,9 342,9 8 10389
15 75 75 289,3 514,3 8 14503
20 100 100 385,7 685,7 8 19989


Travka 50 T-ridge field

Travka 50: T-ridge 2 µm to 6 µm features
Width (µm) Triple width (µm) Area (µm) Space (µm) Total feature width (µm) Number of features Total width (µm)
2 10 10 18,0 48 13 624
3 15 15 27,0 72 12 1488
4 20 20 36,0 96 12 2640
5 25 25 45,0 120 12 4080
6 30 30 54,0 144 12 5808
Travka 50: T-ridge 8 µm to 20 µm features
Width (µm) Triple width (µm) Area (µm) Space (µm) Total feature width (µm) Number of features Total width (µm)
8 40 40 72,0 192 12 8112
10 50 50 90,0 240 11 10752
15 75 75 135,0 360 11 14712
20 100 100 180,0 480 11 19992

Travka 65 T-ridge field

Travka 65: T-ridge 2 µm to 6 µm features
Width (µm) Triple width (µm) Area (µm) Space (µm) Total feature width (µm) Number of features Total width (µm)
2 10 10 6,9 36,9 16 590,8
3 15 15 10,4 55,4 17 1532,3
4 20 20 13,8 73,8 15 2640
5 25 25 17,3 92,3 15 4024,6
6 30 30 20,8 110,8 15 5686,2
Travka 65: T-ridge 8 µm to 20 µm features
Width (µm) Triple width (µm) Area (µm) Space (µm) Total feature width (µm) Number of features Total width (µm)
8 40 40 27,7 147,7 15 7901,5
10 50 50 34,6 184,6 15 10670,8
15 75 75 51,9 276,9 15 14824,6
20 100 100 69,2 369,2 14 19993,8

Travka 80 T-ridge field

Travka 80: T-ridge 2 µm to 6 µm features
Width (µm) Triple width (µm) Area (µm) Space (µm) Total feature width (µm) Number of features Total width (µm)
2 10 10 0 30 18 540
3 15 15 0 45 20 1440
4 20 20 0 60 18 2520
5 25 25 0 75 18 3870
6 30 30 0 90 18 5490
Travka 80: T-ridge 8 µm to 20 µm features
Width (µm) Triple width (µm) Area (µm) Space (µm) Total feature width (µm) Number of features Total width (µm)
8 40 40 0 120 18 7650
10 50 50 0 150 18 10350
15 75 75 0 225 18 14400
20 100 100 0 300 18 19800