'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php?title=Specific_Process_Knowledge/Etch/Wet_III-V_Etches click here]'''  
'''Unless anything else is stated, everything on this page, text and pictures are made by DTU Nanolab.'''


[[Category: Equipment|Etch Wet III-V]]
'''All links to Kemibrug (SDS) and Labmanager Including APV and QC requires login.'''
[[Category: Etch (Wet) bath|III-V]]


This is a collection of III-V wet-etches; the rates should be tested before use. Make sure you have the proper education in mixing of chemicals before use.
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Etch/Wet_III-V_Etches click here]'''


It is utterly important that your dispose of chemicals/etches according to the DTU Danchip regulations; more information is found in the III-V cleanroom.
This is a collection of III-V wet-etches; the rates should be tested before use. Make sure you have the proper education in mixing of chemicals before use. Wet etching of III-V materials is primarily to be done in 'Fume hood 07: III-V acids/bases'. Contact information, risk assessment and manual regarding this fume hood can be found in LabManager:


[http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=374 Fume hood 07 Info page in LabManager]
<br>
<br>
It is very important that you dispose off chemicals and process waste according to DTU Nanolab regulations and risk assessments for your work.


== InP or GaAs substrate etching ==
'''For the GaAs and InP substrate etching, waste should be collected and marked ''Carcinogenic''.
If it contains H2O2 use empty H2O2 bottles (since they should have a special lid that avoid over pressure).
 
There should be waste bottles in the fumehood for citric acid: H2O2 or H2SO4 (10%):H2O2 used to etch GaAs and InGaAsP substrates marked '''"for Carcinogenic materials like InP and GaAs in Acid and Hydrogenperoxide".'''
And one for acid etch of InP marked '''"for Carcinogenic materials like InP and GaAs in Acid - ''NO H2O2"'''
 
This does not apply for etching epilayers.
 
If you need a new bottle, contact Nanolab.
[[Image:FH07.jpg|300x300px|right|thumb|'Fume hood 07' in cleanroom D3]]
<br>
For dry etching III-V materials see
*[[Specific Process Knowledge/Etch/III-V ICP|III-V ICP]]
*[[Specific Process Knowledge/Etch/III-V RIE|III-V RIE - Plassys]] (will be decommissioned October 2025)


When etching InP or GaAs substrates, both 2” wafers and small pieces, you should collect the chemicals used in a waste bottl. This does not apply for etching epilayers.


There should be two bottles in the fumehood one for HCl used to etch InP substrates and one for citric acid: H2O2 or H2SO4 (10%):H2O2 used to etch GaAs substrates.
Once the bottles are full, you should bring them in Danchip basement and have a new one in CR. '''For the GaAs waste you should use empty H2O2 bottles (since they should have a special lid that avoid overpressure)''', while for InP waste we can use an empty and clean developer bottle.


==HCl:H3PO4 etch==
==HCl:H3PO4 etch==


HCl(37%):H<sub>3</sub>PO<sub>4</sub>(85%) is a selective, anisotropic and slow etching of InP. Very slow rate in InGaAsP. The etch rates depend on the orientation of the features and have not yet been calibrated at DTU Danchip.
HCl(37%):H<sub>3</sub>PO<sub>4</sub>(85%) is a selective, anisotropic and slow etching of InP. Very slow rate in InGaAsP. The etch rates depend on the orientation of the features and have not yet been calibrated at DTU Nanolab.


See rates below for InP, PQ(1.n) and InGaAs lattice-matched to InP. '''The acronym PQ(1.n) denotes a lattice-matched InGaAsP on InP with a band gap corresponding to a wavelength of 1.n um.'''  
See rates below for InP, PQ(1.n) and InGaAs lattice-matched to InP. '''The acronym PQ(1.n) denotes a lattice-matched InGaAsP on InP with a band gap corresponding to a wavelength of 1.n um.'''  


The temperature is 22 degC +/- 1 degC.
The temperature is 22 degC +/- 1 degC.
<!-- copyright issue rkc


{| border="1" style="text-align: center; width: 600px; height: 100px;"
{| border="1" style="text-align: center; width: 600px; height: 100px;"
Line 32: Line 45:
! width="20%" |PQ(1.1)
! width="20%" |PQ(1.1)
! width="20%" |InGaAs
! width="20%" |InGaAs
! width="20%" |Contributer
! width="20%" |Contributor
|-
|-
|1:4
|1:4
Line 48: Line 61:


<br>
<br>
-->


==H2SO4:H2O2:H2O etch==
==H2SO4:H2O2:H2O etch==
Line 53: Line 67:
H<sub>2</sub>SO<sub>4</sub>(10%):H<sub>2</sub>O<sub>2</sub>(30%):H<sub>2</sub>O is a selective etch of InGaAsP with very low etch rate in InP. '''The acronym PQ(1.n) denotes a lattice-matched InGaAsP on InP with a band gap corresponding to a wavelength of 1.n um.'''  
H<sub>2</sub>SO<sub>4</sub>(10%):H<sub>2</sub>O<sub>2</sub>(30%):H<sub>2</sub>O is a selective etch of InGaAsP with very low etch rate in InP. '''The acronym PQ(1.n) denotes a lattice-matched InGaAsP on InP with a band gap corresponding to a wavelength of 1.n um.'''  


The etchrates have not yet been calibrated at DTU Danchip.
The etch rates have not yet been calibrated at DTU Nanolab.
The temperature is 22 degC +/- 1 degC.
The temperature is 22 degC +/- 1 degC.
<!-- copyright issue rkc


{| border="1" style="text-align: center; width: 800px; height: 100px;"
{| border="1" style="text-align: center; width: 800px; height: 100px;"
Line 92: Line 108:
|}
|}


'''(1)''' The etchrates have not yet been calibrated at DTU Danchip.
'''(1)''' The etch rates have not yet been calibrated at DTU Nanolab.
-->
<br>
<br>


Line 123: Line 140:
H<sub>3</sub>PO<sub>4</sub>(85%):H<sub>2</sub>O<sub>2</sub>(30%):H<sub>2</sub>O is a GaAs/AlGaAs-etch which gives a better surface quality than H<sub>2</sub>SO<sub>4</sub>-based etches.
H<sub>3</sub>PO<sub>4</sub>(85%):H<sub>2</sub>O<sub>2</sub>(30%):H<sub>2</sub>O is a GaAs/AlGaAs-etch which gives a better surface quality than H<sub>2</sub>SO<sub>4</sub>-based etches.


<!-- copyright issue rkc


{| border="1" style="text-align: center; width: 500px; height: 100px;"
{| border="1" style="text-align: center; width: 500px; height: 100px;"
Line 149: Line 167:


'''(1)''' Temperature of mixture is ~22 degC (no heating during etch). Data is obtained using magnetic stirring with sample on flat basket. '''(2)''' Refrigerated H2O used during mixture of etch, and mixture kept at 17 degC during etch. '''(3)''' 10:2:30 gives smoother etch than 10:2:60.
'''(1)''' Temperature of mixture is ~22 degC (no heating during etch). Data is obtained using magnetic stirring with sample on flat basket. '''(2)''' Refrigerated H2O used during mixture of etch, and mixture kept at 17 degC during etch. '''(3)''' 10:2:30 gives smoother etch than 10:2:60.
-->


<br>
<br>
Line 155: Line 175:


BHF etches SiO<sub>2</sub> and partially removes native oxide on InGaAs and InP. '''Do not use BHF unless you know the dangers involved with this chemical and always use 4H gloves!'''.
BHF etches SiO<sub>2</sub> and partially removes native oxide on InGaAs and InP. '''Do not use BHF unless you know the dangers involved with this chemical and always use 4H gloves!'''.
<!-- copyright issue rkc


{| border="1" style="text-align: center; width: 500px; height: 100px;"
{| border="1" style="text-align: center; width: 500px; height: 100px;"
Line 178: Line 200:
|}
|}


'''(1)''' Ti from Titest.prg on Physimeca. It seems there is no measurable etchig during first 10 seconds.'''(2)''' Process '''SiO2ky2''' in PECVD2 (2014-July Luisa Ottaviamo @photonics ). '''(3)''' Process '''STANDARD''' in PECVD2 (2014-July Luisa Ottaviano @ photonics). '''(4)''' Process '''SINSTD''' in PECVD2 (2014-July Luisa Ottaviano @ photonics). '''(5)''' Appl. Phys. Lett. vol. 51, 2222 (1987).
'''(1)''' Ti from Titest.prg on Physimeca. It seems there is no measurable etching during first 10 seconds.<br>
'''(2)''' Process '''SiO2ky2''' in PECVD2 (2014-July Luisa Ottaviamo @photonics ). <br>
'''(3)''' Process '''STANDARD''' in PECVD2 (2014-July Luisa Ottaviano @ photonics).<br>
'''(4)''' Process '''SINSTD''' in PECVD2 (2014-July Luisa Ottaviano @ photonics). <br>
'''(5)''' Appl. Phys. Lett. vol. 51, 2222 (1987).
<br>
<br>
<br>'''Note:''' neither Physimeca or PECVD2 is available anymore. Use the Temescal and the PECVD3/PECVD4 instead.
-->


==Citric Acid etch==
==Citric Acid etch==
Line 185: Line 214:
C<sub>6</sub>H<sub>8</sub>O<sub>7</sub>:H<sub>2</sub>O<sub>2</sub> is a selective etch of GaAs; does not etch Al<sub>x</sub>Ga<sub>{1-x}</sub>As if x > 0.45.
C<sub>6</sub>H<sub>8</sub>O<sub>7</sub>:H<sub>2</sub>O<sub>2</sub> is a selective etch of GaAs; does not etch Al<sub>x</sub>Ga<sub>{1-x}</sub>As if x > 0.45.


Solid C<sub>6</sub>H<sub>8</sub>O<sub>7</sub> is mixed 1:1 by weight with H<sub>2</sub>O (30%) using magnetic stirring. The solution C<sub>6</sub>H<sub>8</sub>O<sub>7</sub>:H<sub>2</sub>O is thereafter mixed 4:1 volume ratio with H<sub>2</sub>O<sub>2</sub>.
Solid C<sub>6</sub>H<sub>8</sub>O<sub>7</sub> is mixed 1:1 by weight with H<sub>2</sub>O using magnetic stirring. The solution C<sub>6</sub>H<sub>8</sub>O<sub>7</sub>:H<sub>2</sub>O is thereafter mixed 4:1 volume ratio with H<sub>2</sub>O<sub>2</sub>(30%).


The above C<sub>6</sub>H<sub>8</sub>O<sub>7</sub>:H<sub>2</sub>O<sub>2</sub> solution has an etch-rate of ~360 nm/min in GaAs and < 0.5 nm/min in AlAs @ 25 degC.
The above C<sub>6</sub>H<sub>8</sub>O<sub>7</sub>:H<sub>2</sub>O<sub>2</sub> solution has an etch-rate of ~360 nm/min in GaAs and < 0.5 nm/min in AlAs @ 25 degC.
==More info regarding etching of III-V materials==
More info on etching of III-V materials (not the DTU Nanolab wiki) can be found here:
https://wiki.nanofab.ucsb.edu/wiki/Wet_Etching_Recipes '''(at the UCSB Nanofab Wiki)'''
and
https://www.sciencedirect.com/science/article/pii/S0927796X00000279 '''(at the UCSB Nanofab Wiki)'''

Latest revision as of 14:27, 10 February 2026

Unless anything else is stated, everything on this page, text and pictures are made by DTU Nanolab.

All links to Kemibrug (SDS) and Labmanager Including APV and QC requires login.

Feedback to this page: click here

This is a collection of III-V wet-etches; the rates should be tested before use. Make sure you have the proper education in mixing of chemicals before use. Wet etching of III-V materials is primarily to be done in 'Fume hood 07: III-V acids/bases'. Contact information, risk assessment and manual regarding this fume hood can be found in LabManager:

Fume hood 07 Info page in LabManager
It is very important that you dispose off chemicals and process waste according to DTU Nanolab regulations and risk assessments for your work.

For the GaAs and InP substrate etching, waste should be collected and marked Carcinogenic. If it contains H2O2 use empty H2O2 bottles (since they should have a special lid that avoid over pressure).

There should be waste bottles in the fumehood for citric acid: H2O2 or H2SO4 (10%):H2O2 used to etch GaAs and InGaAsP substrates marked "for Carcinogenic materials like InP and GaAs in Acid and Hydrogenperoxide". And one for acid etch of InP marked "for Carcinogenic materials like InP and GaAs in Acid - NO H2O2"

This does not apply for etching epilayers.

If you need a new bottle, contact Nanolab.

'Fume hood 07' in cleanroom D3


For dry etching III-V materials see


HCl:H3PO4 etch

HCl(37%):H3PO4(85%) is a selective, anisotropic and slow etching of InP. Very slow rate in InGaAsP. The etch rates depend on the orientation of the features and have not yet been calibrated at DTU Nanolab.

See rates below for InP, PQ(1.n) and InGaAs lattice-matched to InP. The acronym PQ(1.n) denotes a lattice-matched InGaAsP on InP with a band gap corresponding to a wavelength of 1.n um.

The temperature is 22 degC +/- 1 degC.


H2SO4:H2O2:H2O etch

H2SO4(10%):H2O2(30%):H2O is a selective etch of InGaAsP with very low etch rate in InP. The acronym PQ(1.n) denotes a lattice-matched InGaAsP on InP with a band gap corresponding to a wavelength of 1.n um.

The etch rates have not yet been calibrated at DTU Nanolab. The temperature is 22 degC +/- 1 degC.


Concentrated H2SO4

Concentrated H2SO4(98%) is used for deoxidation of InP with a very low etch rate in InGaAsP.

H2SO4(98%) etch rates, nm/min
Etchant InP PQ(1.1) PQ(1.3) PQ(1.5) InGaAs
H2SO4(98%) 13 ? <1    


H3PO4:H2O2:H2O etch

H3PO4(85%):H2O2(30%):H2O is a GaAs/AlGaAs-etch which gives a better surface quality than H2SO4-based etches.



BHF, HF etch

BHF etches SiO2 and partially removes native oxide on InGaAs and InP. Do not use BHF unless you know the dangers involved with this chemical and always use 4H gloves!.


Citric Acid etch

C6H8O7:H2O2 is a selective etch of GaAs; does not etch AlxGa{1-x}As if x > 0.45.

Solid C6H8O7 is mixed 1:1 by weight with H2O using magnetic stirring. The solution C6H8O7:H2O is thereafter mixed 4:1 volume ratio with H2O2(30%).

The above C6H8O7:H2O2 solution has an etch-rate of ~360 nm/min in GaAs and < 0.5 nm/min in AlAs @ 25 degC.

More info regarding etching of III-V materials

More info on etching of III-V materials (not the DTU Nanolab wiki) can be found here:

https://wiki.nanofab.ucsb.edu/wiki/Wet_Etching_Recipes (at the UCSB Nanofab Wiki)

and

https://www.sciencedirect.com/science/article/pii/S0927796X00000279 (at the UCSB Nanofab Wiki)