Jump to content

Specific Process Knowledge/Thermal Process/Furnace: Multipurpose annealing/Acceptance test: Difference between revisions

From LabAdviser
Pevo (talk | contribs)
Paphol (talk | contribs)
No edit summary
 
(20 intermediate revisions by 3 users not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thermal_Process/Furnace:_Multipurpose_annealing/Acceptance_test  click here]'''


=<span style="background:#FF2800">THIS PAGE IS UNDER CONSTRUCTION</span>[[image:Under_construction.png|200px]]=
''This page is written by DTU Nanolab  internal''


The acceptance for the Multipurpose Anneal furnace was performed in November 2014 by ATV Technologie.
==Multipurpose Anneal furnace acceptance test==


The acceptance for the Multipurpose Anneal furnace was performed in November 2014 by ATV Technologie and DTU Nanolab.


At the acceptance test a dry oxide layer was grown on a boat of 150 mm wafers. The oxide growth was repeated three times


For each run the oxide thickness and refractive index were measured on three of the wafers, and the standard deviation and non-uniformity were calculated for each wafer, over the boat and from run to run.


Recipe: "vr_dryOx_1000C_120min_150_5Wafer_D1_mit_Inliner_oPurgering.ATV"
==Oxidation parameters==


Oxidation time: 80 min
'''Recipe''': "vr_dryOx_1000C_120min_150_5Wafer_D1_mit_Inliner_oPurgering.ATV"
Oxidation temperature: 1050 <sup>o</sup>C
O<sub>2</sub> flow: 1 slm


The oxidation has been done with 150 mm wafer, and with 30 wafers in the furnace.
'''Oxidation time''': 80 min


Wafer 4 (towards the door), wafer 16 and wafer 28 (towards the service area) were measured.
'''Temperature''': 1050 <sup>o</sup>C (all temperature zones)


'''O<sub>2</sub> flow''': 1 slm
The oxidation has been done with 150 mm wafers. The number of wafers in the boat was 30.
Wafer 4 (towards the door), wafer 16 and wafer 28 (towards the service area) were measured in 13 points using the M-2000V ellipsometer.
==Results==
====Oxide thickness====


{| border="2" cellpadding="2" cellspacing="1" style="text-align:center;"
{| border="2" cellpadding="2" cellspacing="1" style="text-align:center;"
|-
|-
! Mask
!  
! Resist etch rate [nm/min]
! Date
! colspan="5" | Silicon etch rate [µm/min]
! colspan="3" | Wafer 4
! colspan="5" | Trench width [µm]
! colspan="3" | Wafer 16
! colspan="5" | Under etch [µm]
! colspan="3" | Wafer 28
! colspan="5" | Silicon etch angle [<sup>o</sup>C]
! colspan="3" | Center point only
|-
|-
! width="80" |   
! width="80" |   
! width="80" |  
! width="80" |  
! width="50" | 2 µm
! width="70" | Average oxide thickness [nm]
! width="50" | 4 µm
! width="70" | St. deviation
! width="50" | 10 µm
! width="70" | Non-uniformity [%]
! width="50" | 50 µm
! width="70" | Average oxide thickness [nm]
! width="50" | 200 µm
! width="70" | St. deviation
! width="50" | 2 µm
! width="70" | Non-uniformity [%]
! width="50" | 4 µm
! width="70" | Average oxide thickness [nm]
! width="50" | 10 µm
! width="70" | St. deviation
! width="50" | 50 µm
! width="70" | Non-uniformity [%]
! width="50" | 200 µm
! width="70" | Average oxide thickness [nm]
! width="50" | 2 µm
! width="70" | St. deviation
! width="50" | 4 µm
! width="70" | Non-uniformity [%]
! width="50" | 10 µm
! width="50" | 50 µm
! width="50" | 200 µm
! width="50" | 2 µm
! width="50" | 4 µm
! width="50" | 10 µm
! width="50" | 50 µm
! width="50" | 200 µm
|-
|-
! Travka5
! Run 1
| 67.31
| 28-01-2015
| 109.7
| 1.0
| 1.7
| 107.7
| 0.9
| 1.1
| 106.5
| 0.8
| 1.2
| 107.0
| 2.1
| 1.9
|-
! Run 2
| 28-01-2015
| 107.3
| 1.7
| 2.4
| 105.0
| 1.4
| 1.7
| 107.3
| 0.7
| 0.9
| 105.7
| 1.0
| 0.9
|-
! Run 3
| 30-01-2015
| 103.6
| 0.8
| 1.1
| 102.6
| 0.6
| 0.6
| 0.63
| 1.2
| 0.63
| 102.2
| 0.62
| 0.6
| 0.61
| 1.1
| 2.60
| 102.9
| 4,91
| 1.0
| 10.96
| 1.0
| 51.00
| 201.90
|
|
|
|
|
|
|
|
|
|
|
|-
|-
! Travka10
! Average
| 63.94
|
| 0.57
| 106.9
| 0.59
| 1.2
| 0.59
| 1.7
| 0.58
| 105.1
| 0.61
| 1.0
| 2.32
| 1.3
| 4.60
| 105.3
| 0.7
|  
| 1.1
|  
| 105.2
|  
| 1.4
|  
| 1.3
|  
|}
|  
 
|
 
|
{| border="2" cellpadding="2" cellspacing="1" style="text-align:center;"
|
|
|
|
|  
|-
|-
! Travka20
! colspan="3" | Run-to-run
| 63.13
| 0.63
| 0.63
| 0.64
| 0.64
| 0.59
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|  
|-
|-
! Travka35
! width="90" | Average oxide thickness [nm]
| 59.63
! width="90" | St. deviation
| 0.57
! width="90" | Non-uniformity [%]
| 0.60
| 0.61
| 0.61
| 0.55
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|  
|-
|-
! Travka50
| 105.2
| 57.13
| 2.1
| 0.47
| 2.0
| 0.5
|}
| 0.51
 
| 0.51
 
| 0.49
====Refractive index====
|  
 
|  
{| border="2" cellpadding="2" cellspacing="1" style="text-align:center;"
|  
|-
|  
!
|  
! Date
|  
! colspan="3" | Wafer 4
|  
! colspan="3" | Wafer 16
|  
! colspan="3" | Wafer 28
|  
! colspan="3" | Center point only
|  
|-
|  
! width="80" | 
|  
! width="80" |
|  
! width="70" | Average refractive index
|  
! width="70" | St. deviation
|  
! width="70" | Non-uniformity [%]
|  
! width="70" | Average refractive index
! width="70" | St. deviation
! width="70" | Non-uniformity [%]
! width="70" | Average refractive index
! width="70" | St. deviation
! width="70" | Non-uniformity [%]
! width="70" | Average refractive index
! width="70" | St. deviation
! width="70" | Non-uniformity [%]
|-
! Run 1
| 28-01-2015
| 1.46
| 0.00
| 0.04
| 1.46
| 0.00
| 0.07
| 1.46
| 0.00
| 0.06
| 1.4609
| 0.0004
| 0.0230
|-
! Run 2
| 28-01-2015
| 1.46
| 0.00
| 0.09
| 1.46
| 0.00
| 0.17
| 1.44
| 0.01
| 0.69
| 1.4561
| 0.0094
| 05873
|-
! Run 3
| 30-01-2015
| 1.46
| 0.00
| 0.06
| 1.46
| 0.00
| 0.05
| 1.46
| 0.00
| 0.07
| 1.4602
| 0.0004
| 0.0291
|-
! Average
|
| 1.46
| 0.00
| 0.06
| 1.46
| 0.00
| 0.10
| 1.46
| 0.00
| 0.27
| 1.46
| 0.00
| 0.21
|}
 
 
{| border="2" cellpadding="2" cellspacing="1" style="text-align:center;"
|-
|-
! Travka65 
! colspan="3" | Run-to-run
| 57.88
| 0.41
| 0.41
| 0.42
| 0.42
| 0.43
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|  
|-
|-
! Travka80 
! width="90" | Average refractive index
| 57.56
! width="90" | St. deviation
| 0.37
! width="90" | Non-uniformity [%]
| 0.36
| 0.37
| 0.37
| 0.38
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|  
|-
|-
! Common
| 1.4591
| colspan="23" | Temperature 20 degs, HBC 10 torr, Short funnel, with baffle & 5mm spacers
| 0.0026
| 0.1637
|}
|}

Latest revision as of 11:28, 2 February 2023

Feedback to this page: click here

This page is written by DTU Nanolab internal

Multipurpose Anneal furnace acceptance test

The acceptance for the Multipurpose Anneal furnace was performed in November 2014 by ATV Technologie and DTU Nanolab.

At the acceptance test a dry oxide layer was grown on a boat of 150 mm wafers. The oxide growth was repeated three times

For each run the oxide thickness and refractive index were measured on three of the wafers, and the standard deviation and non-uniformity were calculated for each wafer, over the boat and from run to run.

Oxidation parameters

Recipe: "vr_dryOx_1000C_120min_150_5Wafer_D1_mit_Inliner_oPurgering.ATV"

Oxidation time: 80 min

Temperature: 1050 oC (all temperature zones)

O2 flow: 1 slm

The oxidation has been done with 150 mm wafers. The number of wafers in the boat was 30.

Wafer 4 (towards the door), wafer 16 and wafer 28 (towards the service area) were measured in 13 points using the M-2000V ellipsometer.

Results

Oxide thickness

Date Wafer 4 Wafer 16 Wafer 28 Center point only
Average oxide thickness [nm] St. deviation Non-uniformity [%] Average oxide thickness [nm] St. deviation Non-uniformity [%] Average oxide thickness [nm] St. deviation Non-uniformity [%] Average oxide thickness [nm] St. deviation Non-uniformity [%]
Run 1 28-01-2015 109.7 1.0 1.7 107.7 0.9 1.1 106.5 0.8 1.2 107.0 2.1 1.9
Run 2 28-01-2015 107.3 1.7 2.4 105.0 1.4 1.7 107.3 0.7 0.9 105.7 1.0 0.9
Run 3 30-01-2015 103.6 0.8 1.1 102.6 0.6 1.2 102.2 0.6 1.1 102.9 1.0 1.0
Average 106.9 1.2 1.7 105.1 1.0 1.3 105.3 0.7 1.1 105.2 1.4 1.3


Run-to-run
Average oxide thickness [nm] St. deviation Non-uniformity [%]
105.2 2.1 2.0


Refractive index

Date Wafer 4 Wafer 16 Wafer 28 Center point only
Average refractive index St. deviation Non-uniformity [%] Average refractive index St. deviation Non-uniformity [%] Average refractive index St. deviation Non-uniformity [%] Average refractive index St. deviation Non-uniformity [%]
Run 1 28-01-2015 1.46 0.00 0.04 1.46 0.00 0.07 1.46 0.00 0.06 1.4609 0.0004 0.0230
Run 2 28-01-2015 1.46 0.00 0.09 1.46 0.00 0.17 1.44 0.01 0.69 1.4561 0.0094 05873
Run 3 30-01-2015 1.46 0.00 0.06 1.46 0.00 0.05 1.46 0.00 0.07 1.4602 0.0004 0.0291
Average 1.46 0.00 0.06 1.46 0.00 0.10 1.46 0.00 0.27 1.46 0.00 0.21


Run-to-run
Average refractive index St. deviation Non-uniformity [%]
1.4591 0.0026 0.1637