| (369 intermediate revisions by 11 users not shown) |
| Line 1: |
Line 1: |
| [[image:Forside20130308 4.jpg|right|500x500px]] | | __notoc__ |
| LabAdviser is a process handbook for equipment and processes at the DTU Danchip cleanroom facilities. The function and capacity of each piece of equipment is described in detail and general process steps, eg photolithography procedures, are clarified. LabAdviser is meant to advise you to a good starting point for your cleanroom process for further optimization to meet your needs. To enter LabAdviser you need to '''log in with your DTU login'''. LabAdviser is only editable for Danchip employees. If you need further information about certain machinery or processes, please contact the Danchip personnel. Any feedback you might have on LabAdviser is welcome and can be given by mail to the LabAdviser mailbox: [mailto:labadviser@danchip.dtu.dk labadviser@danchip.dtu.dk] | | [[image:Til LA forside 2024-05-03 161145.png|right|500x500px|thumb|link=|Photos: DTU Nanolab]] |
| <br>
| | LabAdviser is a Wiki owned by DTU Nanolab for users of our facilities. It was created with the main purpose of sharing knowledge. It contains information about available equipment and fabrication processes in the cleanroom facilities in building 346/347 and the electron microscopes and supporting tools in 307/314/313. |
| | |
|
| |
|
| '''News in LabAdviser:''' <br/>
| | LabAdviser is designed to help you identify the right equipment and provide a solid starting point for your cleanroom processes or for further optimization to meet specific requirements. However, due to ongoing development of tools and processes, some information may be incomplete or not up-to-date. We make every effort to provide reliable information but we provide no warranty as to the accuracy, reliability or completeness of the information found in LabAdviser. |
| The latest monthly LabAdviser update: [[Media:Monthly_LabAdviser_update_20150527.docx|LabAdviser update send out 2015-05-27]] <br>
| |
| Slides from the customer meeting December 2014: [[:File:141216 Kundestormode 2014 final right prices.pdf|Customer meeting 2014]]
| |
| <br/>
| |
|
| |
|
| === Contents ===
| | Please note that LabAdviser is not a replacement for direct communication with DTU Nanolab staff. We strongly recommend reviewing the information on LabAdviser as preparation before reaching out to staff members. |
|
| |
|
| *'''[[Danchip contact information|Danchip contact information]]'''
| | If in doubt, you are always welcome to contact us via [mailto:nanolabsupport@nanolab.dtu.dk nanolabsupport@nanolab.dtu.dk]. |
| *'''[[/Introduction to LabAdviser and Processing|Introduction to LabAdviser and Processing]]'''
| |
| *'''[[/Introduction to LabManager|Introduction to LabManager]]'''
| |
| *'''[[/Process flow approval|Process flow approval]]'''
| |
| *'''[[Specific Process Knowledge]]'''
| |
| *'''[[/Equipment List|Equipment List]]'''
| |
| *'''[[/New equipment in the pipeline and Old equipment for decommissioning|New equipment in the pipeline and old equipment for decommissioning]]'''
| |
| *'''[[Surveys and statistics|Surveys, statistics, monthly LabAdviser updates and other info.]]'''
| |
| *'''[[How to add information to LabAdviser]]'''
| |
| <br clear="all" />
| |
| *'''Overview of processing steps - a guide to where you can find process information in LabAdviser:'''
| |
| {| style="color: black;vertical-align:top" width="100%" border=0 cellpadding="4" cellspacing="0"
| |
| | colspan="2" |
| |
| |-
| |
| | style="width: 50%; vertical-align:top;"|
| |
| {| id="linkTable" border="1" cellpadding="0" cellspacing="0" style="text-align:center;"
| |
| ! class="hideImage" style="display:none"| Front Image
| |
| ! style="display:none"|-
| |
| ! style="display:none"|-
| |
| ! style="display:none"|-
| |
| |-
| |
| ! class="hideImage" width="150" height="180px"| Clean your sample[[file:jehanClean.png|130px|frameless ]]
| |
| ! class="hideImage" width="150" | Dry your sample [[file:jehanDry.png|130px|frameless ]]
| |
| ! class="hideImage" width="150" | Create a thin film on your sample [[file:jehanfilm.png|130px|frameless ]]
| |
| ! class="hideImage" width="150" | Dope your sample [[file:jehanDope.png|130px|frameless ]]
| |
| |-
| |
| ! class="hideImage" width="150" height="180px"| Thermal treatment of your sample [[file:jehanThermal.png|130px|frameless ]]
| |
| ! class="hideImage" width="150" | Make a mask on your sample[[file:jehanmask.png|130px|frameless ]]
| |
| ! class="hideImage" width="150" | Transfer pattern to your sample [[file:jehanTransfer.png|130px|frameless ]]
| |
| ! class="hideImage" width="150" | Define your structure directly [[file:jehandefine.jpg|130px|frameless ]]
| |
| |-
| |
| ! class="hideImage" width="150" height="180px"| Bond your samples together [[file:jehanBond.png|130px|frameless ]]
| |
| ! class="hideImage" width="150" | Characterize your sample [[file:jehanCharacterize.png|130px|frameless ]]
| |
| ! class="hideImage" width="150" | Pack your sample [[file:jehanPack.png|130px|frameless ]]
| |
| ! |
| |
| |-
| |
| |}
| |
|
| |
|
| | style="color:black; width: 50%; vertical-align: top;"|
| | [[Image:Virtual tour in the clean room.JPG|right|300px|thumb|link=https://www.nanolab.dtu.dk/capabilities/cleanroom-3d-tour|Click to Enter the Virtual Tour through DTU Nanolabs cleanroom]] |
| {| class="wikitable hideable hidden" border="1" cellspacing="0" cellpadding="0" align="left" width="430px" style="float:right;"
| |
| ! style="text-align:right;" | [[image:DUV6.jpg|right|400x400px]]
| |
| |- | |
| |} | |
|
| |
|
| | style="color:black; width: 50%; vertical-align: top"|
| | <BR>Even if you are not a current user at our facilities, you are welcome to surf around. Please note that not all information is available without login. You can take a [https://www.nanolab.dtu.dk/capabilities/cleanroom-3d-tour Virtual Tour of the DTU Nanolab cleanroom facility]. Please also take a look at our homepage [https://www.nanolab.dtu.dk/english www.nanolab.dtu.dk] for more information on how to get access and/or collaborate with us as well as our capabilities and research. |
| {| class="wikitable hideable hidden" border="1" cellspacing="0" cellpadding="0" align="left" width="430px"
| |
| ! colspan="3" style="text-align:left;" | [[image:Clean your sample.png|x100px|Clean your sample]] Clean your sample
| |
| |-
| |
| !Entry page in LabAdviser
| |
| !Techniques
| |
| !Materials
| |
| |-
| |
| |rowspan="5" valign="top" |[[Specific Process Knowledge/Wafer cleaning|Wafer cleaning]]
| |
| |Soap Sonic
| |
| |Removes dust and particles
| |
| |-
| |
| |7-up & Piranha
| |
| |Removes traces of organics and alkali ions
| |
| |-
| |
| |RCA
| |
| |Two step process to remove traces of organics and metals
| |
| |-
| |
| |5% HF
| |
| |Removes native oxide
| |
| |-
| |
| |IMEC
| |
| |Removing dust, traces of organics and alkali ions and slightly polish the surface.
| |
| Make the surface hydrophillic
| |
| |-
| |
| |}
| |
| {| class="wikitable hideable hidden" border="1" cellspacing="1" cellpadding="2" align="left" width="430px"
| |
| !colspan="3" style="text-align:left;" | [[image:Dry your sample.png|x100px|Dry your sample]] Dry your sample
| |
| |-
| |
| !Entry page in LabAdviser
| |
| !Techniques
| |
| !Materials
| |
| |-
| |
| |rowspan="4" valign="top" |[[Specific Process Knowledge/Wafer and sample drying|Wafer and sample drying]]
| |
| |Spin dryers
| |
| |Whole wafers
| |
| |-
| |
| |Critial point dryer
| |
| |Sensitive wafers
| |
| |-
| |
| |Ethanol fume drying
| |
| |Sensitive wafers
| |
| |-
| |
| |N2 blow drying
| |
| |N2 pistols
| |
| |-
| |
| |}
| |
| {| class="wikitable hideable hidden" border="1" cellspacing="1" cellpadding="2" align="left" width="600px"
| |
| !colspan="3" style="text-align:left;" | [[image:Create a film on your sample.png|x100px|Create a layer/film on your sample]] Create a layer/film on your sample
| |
| |-
| |
| !Entry page in LabAdviser
| |
| !Techniques
| |
| !Materials
| |
| |-
| |
| |[[Specific Process Knowledge/Thermal Process/Oxidation| Thermal Process/Oxidation]]
| |
| |Thermal oxidation
| |
| |Thermal SiO2
| |
| |-
| |
| |rowspan="8" valign="top"|[[Specific Process Knowledge/Thin film deposition| Thin film deposition]]
| |
| |Sputter deposition
| |
| |Metals: Al, Ti, Cr, Co, Ni, Cu, Mo, Pd, Ag, Sn, Ta, W, Pt, Au, Fe, Mg, Nb, Ru <br>
| |
| Semiconductors: Si, Ge, ZnO <br>
| |
| Oxides: SiO<sub>2</sub>, ITO, TiO<sub>2</sub>, Al<sub>2</sub>O<sub>3</sub>, MgO, Ta<sub>2</sub>O<sub>5</sub> Cr<sub>2</sub>O<sub>3</sub><br>
| |
| Transparent Conducting Oxides: ITO, AZO<br>
| |
| Alloys: TiW, NiCr, AlTi, NiV, AlCu, CoFe, CuTi, FeMn, MnIr, NiCo, NiFe, YSZ <br>
| |
| |-
| |
| |Thermal evaporation
| |
| |Al, Ge, Ag
| |
| |-
| |
| |E-beam evaporation
| |
| |Metals: Ti, Cr, Al, Ni, Pt, Au, Mo, Pd, Ag, Cu, W, Ta <br>
| |
| Semiconductors: Si, Ge <br>
| |
| Oxides: SiO<sub>2</sub>, TiO<sub>2</sub> <br>
| |
| Alloys: NiCr, TiAl
| |
| |-
| |
| |LPCVD
| |
| |Si<sub>3</sub>N<sub>4</sub>, SRN, SiO<sub>2</sub>, Si (poly and amorph)
| |
| |-
| |
| |PECVD
| |
| |Si<sub>3</sub>N<sub>4</sub>, SiO<sub>2</sub>, PBSG
| |
| |-
| |
| |MVD
| |
| |FDTS
| |
| |-
| |
| |Electroplating
| |
| |Ni
| |
| |-
| |
| |Epitaxial growth /MOCVD
| |
| |Al, As, Ga, In, P. doping: Si, Zn
| |
| |-
| |
| |rowspan="2" valign="top"| [[Specific Process Knowledge/Lithography/Coaters|Lithography/Coaters]]
| |
| |Spin coating
| |
| |resists, polymers
| |
| |-
| |
| |Spray coating
| |
| |resists, polymers
| |
| |-
| |
| |}
| |
| {| class="wikitable hideable hidden" border="1" cellspacing="1" cellpadding="2" align="left" width="430px"
| |
| !colspan="3" style="text-align:left;" | [[image:Dope your sample.png|x100px|Dope your sample]] Dope your sample
| |
| |-
| |
| |-
| |
| !Entry page in LabAdviser
| |
| !Techniques
| |
| !Materials
| |
| |-
| |
| |rowspan="5" valign="top"| [[Specific Process Knowledge/Doping|Doping]]
| |
| |Ion implant
| |
| |e.g. P, B, As
| |
| |-
| |
| |[[Specific Process Knowledge/Thin film deposition/PECVD| PECVD]]
| |
| |Deposition of SiO2 or Si3N4 doped with P,B and Ge
| |
| |-
| |
| |[[Specific Process Knowledge/Thin film deposition/Furnace LPCVD PolySilicon|LPCVD ]]
| |
| |Deposition of PolySi doped with B or P
| |
| |-
| |
| |[[Specific Process Knowledge/Thermal Process/Dope with Boron|Predeposition and drive-in]]
| |
| |Doping Silicon wafers with boron
| |
| |-
| |
| |[[Specific Process Knowledge/Thermal Process/Dope with Phosphorus|Predeposition and drive-in]]
| |
| |Doping Silicon wafers with phosphorus
| |
|
| |
|
| |-
| | [[Image:YouTube.JPG|right|300px|thumb|link=https://www.youtube.com/@dtunanolab1398|Click to Visit DTU Nanolab on YouTube ]] |
| |}
| |
| {| class="wikitable hideable hidden" border="1" cellspacing="1" cellpadding="2" align="left" width="430px"
| |
| !colspan="3" style="text-align:left;" | [[image:Thermal treat your sample.png|x100px|Thermal treatment of your sample]] Thermal treatment of your sample
| |
| |- | |
| !Entry page in LabAdviser
| |
| !Techniques
| |
| !Materials
| |
| |- | |
| |rowspan="5" valign="top"|[[Specific Process Knowledge/Thermal Process|Thermal Process]] | |
| |Annealing (>350C)
| |
| |Si, PECVD layers, Al, BCB curing, Polymer
| |
| |-
| |
| |Oxidation
| |
| |Si wafers
| |
| |-
| |
| |Doping with B/P
| |
| |Si wafers
| |
| |-
| |
| |Pyrolysis
| |
| |Resists: AZ, SU8, PDMS
| |
| |-
| |
| |Rapid Thermal Anneal (RTP)
| |
| |SiO2, Si3N4, Ti, III-V
| |
| |-
| |
| |
| |
| [[Specific Process Knowledge/Lithography/Baking| Lithography/Baking]] <br>
| |
| |Baking (<300dg)
| |
| |baking resist and polymers
| |
| |-
| |
| |}
| |
| {| class="wikitable hideable hidden" border="1" cellspacing="1" cellpadding="2" align="left" width="430px"
| |
| !colspan="3" style="text-align:left;" | [[image:Make a mask on your sample.png|x100px|Make a mask on your sample]] Make a mask on your sample
| |
| |-
| |
| !Entry page in LabAdviser
| |
| !Techniques
| |
| !Materials
| |
| |-
| |
| |rowspan="5" valign="top"|[[Specific Process Knowledge/Lithography| Lithography]]
| |
| |Pattern design & Mask fabrication
| |
| |
| |
| |-
| |
| |Photolithography
| |
| |UV resists
| |
| |-
| |
| |Deep UV lithography
| |
| |DUV resists
| |
| |-
| |
| |E-beam lithography
| |
| |E-beam resists
| |
| |-
| |
| |Imprinting
| |
| |Polymers
| |
| |-
| |
| |}
| |
| {| class="wikitable hideable hidden" border="1" cellspacing="1" cellpadding="2" align="left" width="430px"
| |
| !colspan="3" style="text-align:left;" | [[image:Transfer mask pattrn to your sample.png|x100px|Transfer mask pattern to your sample]] Transfer mask pattern to your sample
| |
| |-
| |
| !Entry page in LabAdviser
| |
| !Techniques
| |
| !Materials
| |
| |-
| |
| |rowspan="2" valign="top"|[[Specific Process Knowledge/Etch| Etch]]
| |
| |Wet etch
| |
| |Si, Glass, SiO2, Si3N4, Al, Cr, Ti, Au, Pt, InP, InGaAsP, GaAs/AlGaAs
| |
| |-
| |
| |Dry etch
| |
| |Any material
| |
| |-
| |
| |[[Specific Process Knowledge/Lithography/LiftOff| Lithography/Lift-off]]
| |
| |Lift-off
| |
| |Most materials
| |
| |-
| |
| |}
| |
| {| class="wikitable hideable hidden" border="1" cellspacing="1" cellpadding="2" align="left" width="430px"
| |
| !colspan="3" style="text-align:left;" | [[image:Define your structure directly.png|x100px|Define the structure directly on your sample]] Define your structure directly
| |
| |-
| |
| !Entry page in LabAdviser
| |
| !Techniques
| |
| !Materials
| |
| |-
| |
| |rowspan="5" valign="top"|[[Specific Process Knowledge/Direct Structure Definition|Direct Structure Definition]]
| |
| |Polymer Injection molding
| |
| |Topas, PP, PE, PS
| |
| |-
| |
| |LASER micro machining
| |
| |Silicon, Metal, Graphene (on silicon), Glass (Pyrex, fused silica), TOPAS, PMMA
| |
| |-
| |
| |Dicing saw
| |
| |Silicon, Glass (Pyrex, fused silica)
| |
| |-
| |
| |[[Specific Process Knowledge/Imprinting|Imprinting]]
| |
| |TOPAS, PMMA
| |
| |-
| |
| |[[Specific Process Knowledge/Lithography|Lithography definition]]
| |
| |SU8, AZ resists
| |
| |-
| |
| |}
| |
| {| class="wikitable hideable hidden" border="1" cellspacing="1" cellpadding="2" align="left" width="430px"
| |
| !colspan="3" style="text-align:left;" | [[image:Bond your samples together.png|x100px|Bond your samples together]] Bond your samples together
| |
| |-
| |
| !Entry page in LabAdviser
| |
| !Techniques
| |
| |-
| |
| |rowspan="3" valign="top"|[[Specific Process Knowledge/Bonding|Bonding]]
| |
| |Eutectic bonding
| |
| |-
| |
| |Fusion bonding
| |
| |-
| |
| |Anodic bonding
| |
| |-
| |
| |[[Specific_Process_Knowledge/Etch/DryEtchProcessing/Bonding |Etch/DryEtchProcessing/Bonding]]
| |
| |Temporary bonding of wafers or chips for dry etching
| |
| |-
| |
| |}
| |
| {| class="wikitable hideable hidden" border="1" cellspacing="1" cellpadding="2" align="left" width="430px"
| |
| !colspan="3" style="text-align:left;" | [[image:Characterize your sample.png|x100px|Characterize your sample]] Characterize your sample
| |
| |-
| |
| !Entry page in LabAdviser
| |
| !What do you need to measure?
| |
| !Technique/Method
| |
| |-
| |
| |rowspan="12" valign="top"|[[Specific Process Knowledge/Characterization|Characterization]]
| |
| |Sample Imaging, XY dimensions
| |
| |Microscopy: optical, SEM, AFM
| |
| |-
| |
| |Sample Topography
| |
| |AFM, Profiling with stylus or optical
| |
| |-
| |
| |Film thickness and optical constants
| |
| |Ellipsometry, Reflectometry, Prism Coupling
| |
| |-
| |
| |Film Stress
| |
| |Profiling with stylus or optical
| |
| |-
| |
| |Wafer thickness
| |
| |Micrometer gauge
| |
| |-
| |
| |Element analysis
| |
| |XPS, EDX, SIMS
| |
| |-
| |
| |Contact Angle
| |
| |Drop shape analyzing
| |
| |-
| |
| |Resistivity
| |
| |Four point probe, Probe station
| |
| |-
| |
| |Doping level/Carrier density
| |
| |ECV (Electrochemical Capacitance-Voltage) -profiler
| |
| |-
| |
| |Direct Bandgap
| |
| |Photoluminescence
| |
| |-
| |
| |Lattice mismatch
| |
| |X-ray diffractometer
| |
| |-
| |
| |Defects/contamination
| |
| |Particle/defect counter
| |
| |-
| |
| |}
| |
| {| class="wikitable hideable hidden" border="1" cellspacing="1" cellpadding="2" align="left" width="430px"
| |
| !colspan="3" style="text-align:left;" | [[image:Pack your sample (back-end).png|x100px|Pack your sample (back-end)]] Pack your sample (back-end)
| |
| |-
| |
| !Entry page in LabAdviser
| |
| !Techniques
| |
| |-
| |
| |rowspan="3" valign="top"|[[Specific Process Knowledge/Back-end processing|Back-end processing]]
| |
| |Chip/die mounting
| |
| |-
| |
| |Wire bonding
| |
| |-
| |
| |Dicing
| |
| |-
| |
| |}
| |
| |
| |
| |-
| |
| |}
| |
|
| |
|
| ---- | | You are also welcome to explore our [https://www.youtube.com/channel/UCJhdUTUJRDNODNiC3V95RQQ YouTube channel] with a selection of training videos. |
| | <BR><BR><br> |
| | '''LabAdviser contains information about''' |
| | *Equipment available in- and outside of the Cleanroom Facility (building 346) |
| | *Equipment for Characterization, primarily Electron Microscopy (building 314 and 307) |
| | *Equipment available in the PolyFabLab and SupportLab (building 347) |
| | *Processes for Micro- and Nanofabrication available at DTU Nanolab |
| | *Methods in Electron Microscopy available in building 314/307 |
| <br> | | <br> |
|
| |
| == Danchip Contact Info ==
| |
| {{DanchipInfo}}
| |
| ----
| |
| <br> | | <br> |
| | ==How Labadviser works== |
|
| |
|
| ==Cleanroom naming and phone numbers==
| | Among others information, Labadviser offers users nano- and microfabrication information on how to build up a process flow, f.ex. |
| | how to create a pattern, what materials to use, what process or equipment to use, how to avoid cross contamination between machines, or how to clean samples. |
|
| |
|
| {| style="color: black;" width="100%"
| | The structure of LabAdviser allows users to begin their search either from a known process. For example, if your process involves depositing a gold layer, you would start with the "Thin Film Deposition" section. There, you will find two tables: |
| | colspan="2" |
| |
| |-
| |
|
| |
|
| | style="width: 50%"|
| | * Overview of '''Materials''', ''such semiconductors, oxides, nitrides, metals, etc.'' |
| | * Overview over '''Thin Film Deposition Equipment''', ''such as thermal evaporator, e-beam evaporator, sputter coater, etc.'' |
|
| |
|
| {| style="color: black;" width="100%"
| | If you know the material you want to deposit but are unsure which tool to use or how different deposition methods compare, you can select the material (e.g. ''gold''). You will then be directed to a subpage listing all equipment capable of depositing that material and, if available, with some additional material-specific process information. |
| | colspan="2" |
| |
| |-
| |
| | style="width: 40%"|
| |
|
| |
|
| | Alternatively, if you're more interested in a specific piece of equipment, or wish to explore which materials it can process, selecting that equipment will lead you to a dedicated page with detailed process information, including compatible materials.<BR> |
| | <br> |
| | <br> |
| | ==How to add Information to Labadviser== |
|
| |
|
| [[image:cleanroom naming 2014.jpg|500px]]
| | Sharing knowledge is the key for further development and all our users are encouraged to contribute. In our laboratories thousands of experiments are made. We want to make sure that the knowledge and experience acquired through these become accessible to current and future users. We are interested in any process development being done on our equipment, and even single tests of new recipes can be helpful. For the safety of our users as well as our equipment, we cannot allow LabAdviser to have an open-for-all-input structure like Wikipedia. |
|
| |
|
| |}
| | We are committed to giving proper credit to all contributors. If you provide material for publication in Labadviser, you will be clearly acknowledged as the author or source. Before publishing your material, we will request your written permission to do so. This ensures transparency and respect for your rights as a creator. More information regarding copyrights can be found [[LabAdviser:Copyright | <b>here</b>]]. |
| | style="width: 50%"|
| |
|
| |
|
| | Any feedback or input is welcome and can be send to the LabAdviser mailbox: [mailto:labadviser@nanolab.dtu.dk labadviser@nanolab.dtu.dk]. |
| | <br> |
| | <br> |
|
| |
|
| {|border="1" cellspacing="1" cellpadding="1" style="text-align:left;"
| | == Surveys and Statistics == |
| |-
| | '''Surveys''' |
|
| |
|
| |-
| | DTU Nanolab performs regular customer surveys which are available on LabManager. ''Access to LabManager requires a DTU account and access to DTU Nanolab facilities.'' |
| |-style="background:silver; color:black"
| |
| !Room number
| |
| !Where in the room
| |
| !Phone number
| |
| |-
| |
|
| |
|
| |-
| | [https://labmanager.dtu.dk/function.php?module=CustomerSurvey&view=show&scope_id=2 Bld.314/307] |
| |-style="background:WhiteSmoke; color:black"
| | <BR> |
| !A-1
| | [https://labmanager.dtu.dk/function.php?module=CustomerSurvey&view=show&scope_id=1 Bld.346/347] |
| |At III-V RIE
| |
| |55 804
| |
| |-
| |
|
| |
|
| |-
| |
| |-style="background:WhiteSmoke; color:black"
| |
| !Ax2
| |
| |At the Lesker
| |
| |55 815
| |
| |-
| |
|
| |
|
| |-
| | '''Tech Forum slides''' |
| |-style="background:LightGrey; color:black"
| |
| !A-5
| |
| |In the corner near the furnace/plasma asher
| |
| |55 803
| |
| |-
| |
| |-
| |
| |-style="background:LightGrey; color:black"
| |
| !B-1
| |
| |In the corridor
| |
| |55 806
| |
| |-
| |
|
| |
|
| |-
| | The purpose of the Nanolab Technology Forum is to discuss the current and future technological possibilities at Nanolab, including user requirements, current equipment status, equipment acquisition, funding, etc. |
| |-style="background:WhiteSmoke; color:black"
| | <!--If you wish to receive the meeting invitation, please sign up beneath. |
| !C-1 | | !--> |
| |At the corridor
| |
| |55 808
| |
| |-
| |
|
| |
|
| |-
| | Tech Forum slides are available on LabManager. ''Access to LabManager requires a DTU account and access to DTU Nanolab facilities.'' |
| |-style="background:LightGrey; color:black"
| |
| !D-1
| |
| |The entrance room
| |
| |55 703
| |
| |-
| |
|
| |
|
| |-
| | [https://labmanager.dtu.dk/function.php?module=PeriodicDocument&view=docs&page_id=397 Tech Forum Slides] |
| |-style="background:WhiteSmoke; color:black"
| | <br> |
| !D-3
| | <br> |
| |At the KOH
| |
| |55 940
| |
| |-
| |
| | |
| |-
| |
| |-style="background:LightGrey; color:black"
| |
| !E-1
| |
| |By the thin client
| |
| |55 943
| |
| |-
| |
| | |
| |-
| |
| |-style="background:WhiteSmoke; color:black"
| |
| !E-5
| |
| |By Inclined UV-lamp
| |
| |55 946
| |
| |-
| |
| | |
| |-
| |
| |-style="background:LightGrey; color:black"
| |
| !E-6
| |
| |Furnace 6"
| |
| |55 948
| |
| |-
| |
| |-
| |
| |-style="background:WhiteSmoke; color:black"
| |
| !F-1
| |
| |III-V growth
| |
| |55 949
| |
| |-
| |
| | |
| |-
| |
| |-style="background:LightGrey; color:black"
| |
| !F-2
| |
| |Opposite SEM Zeiss
| |
| |55 941
| |
| |-
| |
| |-
| |
| |-style="background:WhiteSmoke; color:black"
| |
| !F-3
| |
| |DUV Stepper
| |
| |55 947
| |
| |-
| |
| | |
| |-
| |
| |-style="background:LightGrey; color:black"
| |
| !SIMS/XPS room in the basement
| |
| |?
| |
| |55 813
| |
| |-
| |
| |-
| |
| |-style="background:WhiteSmoke; color:black"
| |
| !Injection molder room in the basement
| |
| |?
| |
| |55 812
| |
| |-
| |
| |}
| |
| |}
| |
| <br clear="all" /> | |