'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_Film_deposition/ALD/TiO2_deposition_using_ALD click here]''' | |||
<br> | |||
<br> | |||
The ALD window for titanium dioxide (TiO<sub>2</sub>) ranges from 120 <sup>o</sup>C to 350 <sup>o</sup>C. | The ALD window for titanium dioxide (TiO<sub>2</sub>) ranges from 120 <sup>o</sup>C to 350 <sup>o</sup>C. | ||
A low temperatures between 120 <sup>o</sup>C and 150 <sup>o</sup>C an | A low temperatures between 120 <sup>o</sup>C and 150 <sup>o</sup>C an amorphous TiO<sub>2</sub> layer is grown in the ALD, and at higher temperatures between 300 <sup>o</sup>C and 350 <sup>o</sup>C an anatase TiO<sub>2</sub> layer is grown. At temperatures between 150 <sup>o</sup>C and 300 <sup>o</sup>C the TiO<sub>2</sub> layer will be a mixture of both amorphous and anatase TiO<sub>2</sub>. | ||
For Si wafers, amorphous TiO<sub>2</sub> is best grown on wafers with native oxide, and anatase TiO<sub>2</sub> is best grown on wafers without native oxide (removed using HF). | |||
====TiO<sub>2</sub> standard recipe==== | |||
<b>Recipe</b>: TiO2 | <b>Recipe</b>: TiO2 | ||
<b>Temperature</b>: | <b>Temperature</b>: 120 <sup>o</sup>C - 350 <sup>o</sup>C | ||
{| border="2" cellspacing="2" cellpadding="5" align="none" | {| border="2" cellspacing="2" cellpadding="5" align="none" | ||
|- | |- | ||
| | | | ||
! | !TiCl<sub>4</sub> | ||
!H<sub>2</sub>O | !H<sub>2</sub>O | ||
|- | |- | ||
| Line 40: | Line 33: | ||
|- | |- | ||
!Purge time | !Purge time | ||
|4.0 s | |4.0 s | ||
|5.0 s | |||
|- | |- | ||
|} | |} | ||
====TiO<sub>2</sub> deposition rates==== | |||
In the graphs below the TiO<sub>2</sub> thickness as function of number of cycles for deposition temperatures between 150 <sup>o</sup>C and 350 <sup>o</sup>C can be seen. From the equations the number of cycles required for a certain thickess can be calculated. | In the graphs below the TiO<sub>2</sub> thickness as function of the number of cycles for deposition temperatures between 150 <sup>o</sup>C and 350 <sup>o</sup>C can be seen. From the equations the number of cycles required for a certain thickess to be deposited can be calculated. All results have been obtained for Si wafers with native oxide. | ||
<gallery caption="Titanium | <gallery caption="Titanium dioxide thickness as function of number of cycles" widths="300px" heights="300px" perrow="3"> | ||
image:ALD_TiO2_grow_rate_150C.jpg| Temperature 150 <sup>o</sup>C. | image:ALD_TiO2_grow_rate_150C.jpg| Temperature 150 <sup>o</sup>C. | ||
image:ALD_TiO2_grow_rate_250C.jpg| Temperature | image:ALD_TiO2_grow_rate_250C.jpg| Temperature 250 <sup>o</sup>C. | ||
image:ALD_TiO2_grow_rate_350C.jpg| Temperature 250 <sup>o</sup>C. | image:ALD_TiO2_grow_rate_350C.jpg| Temperature 350 <sup>o</sup>C. | ||
</gallery> | |||
Evgeniy Shkondin, DTU Nanolab (former DTU Danchip), April-May 2014. | |||
====TiO<sub>2</sub> results==== | |||
Some some SEM images of TiO<sub>2</sub> deposited on a Si surface at different temperatures between 150 <sup>o</sup>C and 350 <sup>o</sup>C are shown below. Some of samples have been treated with HF (hydrofluoric acid) to remove the native oxide layer just before the ALD deposition. | |||
<gallery caption="Titanium dioxide deposited at different temperatures on a Si surface" widths="250px" heights="180px" perrow="3"> | |||
image:TiO2 150C 1200 cycles Si_HF_treated.jpg| Temperature 150 <sup>o</sup>C, 1200 cycles, HF treated. | |||
image:TiO2 150C 1200 cycles Si_untreated.jpg| Temperature 150 <sup>o</sup>C, 1200 cycles. | |||
image:TiO2 250C 750cycles_Si_untreated.jpg| Temperature 250 <sup>o</sup>C, 750 cycles. | |||
</gallery> | |||
<gallery caption="" widths="250px" heights="180px" perrow="5"> | |||
image:TiO2 1000 cycles 300C Si_HF.jpg| Temperature 300 <sup>o</sup>C, 1000 cycles, HF treated. | |||
image:TiO2 1000 cycles 300C Si_un.jpg| Temperature 300 <sup>o</sup>C, 1000 cycles. | |||
image:TiO2 350C 1250 cycles Si_HF_treated.jpg| Temperature 350 <sup>o</sup>C, 1250 cycles, HF treated. | |||
</gallery> | </gallery> | ||
XPS measurements of TiO<sub>2</sub> deposited at 120 <sup>o</sup>C and 300 <sup>o</sup>C are shown below. From the XPS measurements it can be calculated that at temperatures below 120 <sup>o</sup>C the TiO<sub>2</sub> layer will be contaminated with about 1-3 % chlorine molecules from the TiCl<sub>4</sub> precursor. This can be also seen as small white dots in the SEM image of the amorphous TiO<sub>2</sub> layers above. | |||
[[image:XPS_TiO2.jpg|320x320px|left|thumb|XPS measurements of titanium dioxide.]] | |||
<br clear="all" /> | |||
Evgeniy Shkondin, DTU Nanolab (former DTU Danchip), 2014. | |||
====TiO<sub>2</sub> deposition on trenches==== | |||
For TiO<sub>2</sub> deposition on trenches more information can be found here: | |||
*[[Specific Process Knowledge/Thin Film deposition/ALD/TiO2 deposition using ALD/TiO2 deposition on trenches using ALD|TiO<sub>2</sub> deposition on trenches using ALD]] | |||