Jump to content

Specific Process Knowledge/Thin Film deposition/ALD/TiO2 deposition using ALD: Difference between revisions

Pevo (talk | contribs)
No edit summary
Mmat (talk | contribs)
mNo edit summary
 
(35 intermediate revisions by 4 users not shown)
Line 1: Line 1:
=<span style="background:#FF2800">THIS PAGE IS UNDER CONSTRUCTION</span>[[image:Under_construction.png|200px]]=
{{cc-nanolab}}
 
 
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Thin_Film_deposition/ALD/TiO2_deposition_using_ALD click here]'''


'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_Film_deposition/ALD/TiO2_deposition_using_ALD click here]'''
<br>
<br>
The ALD window for titanium dioxide (TiO<sub>2</sub>) ranges from 120 <sup>o</sup>C to 350 <sup>o</sup>C.  
The ALD window for titanium dioxide (TiO<sub>2</sub>) ranges from 120 <sup>o</sup>C to 350 <sup>o</sup>C.  


A low temperatures between 120 <sup>o</sup>C and 150 <sup>o</sup>C an anatase TiO<sub>2</sub> layer is grow in the ALD, and at higher temperatures between 300 <sup>o</sup>C and 350 <sup>o</sup>C and amorphous TiO<sub>2</sub> layer is grown in the ALD. At temperatures between 150 <sup>o</sup>C and 300 <sup>o</sup>C the TiO<sub>2</sub> layer will be a mixture of both anatase and amorphous TiO<sub>2</sub>.
A low temperatures between 120 <sup>o</sup>C and 150 <sup>o</sup>C an amorphous TiO<sub>2</sub> layer is grown in the ALD, and at higher temperatures between 300 <sup>o</sup>C and 350 <sup>o</sup>C an anatase TiO<sub>2</sub> layer is grown. At temperatures between 150 <sup>o</sup>C and 300 <sup>o</sup>C the TiO<sub>2</sub> layer will be a mixture of both amorphous and anatase TiO<sub>2</sub>.
 
SEM images of both anatase and amorphous TiO<sub>2</sub> are shown below.
 
For Si wafers, anatase TiO<sub>2</sub> is best grown wafers without native oxide (do an BHF etch), and amorphous TiO<sub>2</sub> is best grown on wafers with native oxide.


XPS measurements shows that at temperaturs below 120 <sup>o</sup>C the TiO<sub>2</sub> layer will be contaminated by Cl molecules from the TiCl<sub>4</sub> precursor.
For Si wafers, amorphous TiO<sub>2</sub> is best grown on wafers with native oxide, and anatase TiO<sub>2</sub> is best grown on wafers without native oxide (removed using HF).






 
====TiO<sub>2</sub> standard recipe====
 
All results shown on this page have been obtained using the "TiO2" recipe on new Si(100) wafers with native oxide:
 


<b>Recipe</b>: TiO2
<b>Recipe</b>: TiO2


<b>Temperature</b>: 150 <sup>o</sup>C - 350 <sup>o</sup>C
<b>Temperature</b>: 120 <sup>o</sup>C - 350 <sup>o</sup>C


{| border="2" cellspacing="2" cellpadding="5"  align="none"
{| border="2" cellspacing="2" cellpadding="5"  align="none"
|-  
|-  
|
|
!TMA
!TiCl<sub>4</sub>
!H<sub>2</sub>O
!H<sub>2</sub>O
|-
|-
Line 40: Line 33:
|-  
|-  
!Purge time
!Purge time
|3.0 s
|4.0 s
|4.0 s
|5.0 s
|-
|-
|}
|}




====TiO<sub>2</sub> deposition rates====


In the graphs below the TiO<sub>2</sub> thickness as function of number of cycles for deposition temperatures between 150 <sup>o</sup>C and 350 <sup>o</sup>C can be seen. From the equations the number of cycles required for a certain thickess can be calculated.  
In the graphs below the TiO<sub>2</sub> thickness as function of the number of cycles for deposition temperatures between 150 <sup>o</sup>C and 350 <sup>o</sup>C can be seen. From the equations the number of cycles required for a certain thickess to be deposited can be calculated. All results have been obtained for Si wafers with native oxide. 


<gallery caption="Titanium oxide thickness as function of number of cycles" widths="220px" heights="220px" perrow="5">
<gallery caption="Titanium dioxide thickness as function of number of cycles" widths="300px" heights="300px" perrow="3">
image:ALD_TiO2_grow_rate_150C.jpg| Temperature 150 <sup>o</sup>C.
image:ALD_TiO2_grow_rate_150C.jpg| Temperature 150 <sup>o</sup>C.
image:ALD_TiO2_grow_rate_250C.jpg| Temperature 200 <sup>o</sup>C.
image:ALD_TiO2_grow_rate_250C.jpg| Temperature 250 <sup>o</sup>C.
image:ALD_TiO2_grow_rate_350C.jpg| Temperature 250 <sup>o</sup>C.
image:ALD_TiO2_grow_rate_350C.jpg| Temperature 350 <sup>o</sup>C.
</gallery>
 
Evgeniy Shkondin, DTU Nanolab (former DTU Danchip), April-May 2014.
 
 
====TiO<sub>2</sub> results====
 
Some some SEM images of TiO<sub>2</sub> deposited on a Si surface at different temperatures between 150 <sup>o</sup>C and 350 <sup>o</sup>C are shown below. Some of samples have been treated with HF (hydrofluoric acid) to remove the native oxide layer just before the ALD deposition.
 
<gallery caption="Titanium dioxide deposited at different temperatures on a Si surface" widths="250px" heights="180px" perrow="3">
image:TiO2 150C 1200 cycles Si_HF_treated.jpg| Temperature 150 <sup>o</sup>C, 1200 cycles, HF treated.
image:TiO2 150C 1200 cycles Si_untreated.jpg| Temperature 150 <sup>o</sup>C, 1200 cycles.
image:TiO2 250C 750cycles_Si_untreated.jpg| Temperature 250 <sup>o</sup>C, 750 cycles.
</gallery>
<gallery caption="" widths="250px" heights="180px" perrow="5">
image:TiO2 1000 cycles 300C Si_HF.jpg| Temperature 300 <sup>o</sup>C, 1000 cycles, HF treated.
image:TiO2 1000 cycles 300C Si_un.jpg| Temperature 300 <sup>o</sup>C, 1000 cycles.
image:TiO2 350C 1250 cycles Si_HF_treated.jpg| Temperature 350 <sup>o</sup>C, 1250 cycles, HF treated.
</gallery>
</gallery>
XPS measurements of TiO<sub>2</sub> deposited at 120 <sup>o</sup>C and 300 <sup>o</sup>C are shown below. From the XPS measurements it can be calculated that at temperatures below 120 <sup>o</sup>C the TiO<sub>2</sub> layer will be contaminated with about 1-3 % chlorine molecules from the TiCl<sub>4</sub> precursor. This can be also seen as small white dots in the SEM image of the amorphous TiO<sub>2</sub> layers above.
[[image:XPS_TiO2.jpg|320x320px|left|thumb|XPS measurements of titanium dioxide.]]
<br clear="all" />
Evgeniy Shkondin, DTU Nanolab (former DTU Danchip), 2014.
====TiO<sub>2</sub> deposition on trenches====
For TiO<sub>2</sub> deposition on trenches more information can be found here:
*[[Specific Process Knowledge/Thin Film deposition/ALD/TiO2 deposition using ALD/TiO2 deposition on trenches using ALD|TiO<sub>2</sub> deposition on trenches using ALD]]