Jump to content

Specific Process Knowledge/Etch/DRIE-Pegasus/showerheadchange/ProcessD/PrD01: Difference between revisions

From LabAdviser
Jmli (talk | contribs)
Created page with " {| border="2" cellpadding="0" cellspacing="0" style="text-align:center;" |+ '''Process runs''' |- ! rowspan="2" width="40"| Date ! colspan="4" width="120"| Substrate Informat..."
 
Jmli (talk | contribs)
No edit summary
 
(7 intermediate revisions by the same user not shown)
Line 1: Line 1:
<!--Checked for updates on 11/2-2019 - ok/jmli -->
<!--Page reviewed by jmli 9/8-2022  -->
<!--Checked for updates on 6/2-2013 - ok/jmli -->
{{Template:Author-jmli1}}
<!--Checked for updates on 4/9-2025 - ok/jmli -->


{| border="2" cellpadding="0" cellspacing="0" style="text-align:center;"
{| border="2" cellpadding="0" cellspacing="0" style="text-align:center;"
Line 23: Line 28:
| Pegasus/jmli
| Pegasus/jmli
| 10 minute TDESC clean
| 10 minute TDESC clean
| danchip/jml/showerhead/prD/PrD01, 110 cyc or 6:14 mins
| nanolab/jml/showerhead/prD/PrD01, 110 cyc or 6:14 mins
| S004691
| S004691
! New showerhead  
! New showerhead  
|  
|  
 
[[file:S004691-04.jpg|150px|frameless ]]
[[file:S004691-05.jpg|150px|frameless ]]
[[file:S004691-06.jpg|150px|frameless ]]
[[file:S004691-07.jpg|150px|frameless ]]
[[file:S004691-08.jpg|150px|frameless ]]
[[file:S004691-01.jpg|150px|frameless ]]
[[file:S004691-02.jpg|150px|frameless ]]
[[file:S004691-03.jpg|150px|frameless ]]
|-
|-
|}
|}

Latest revision as of 10:30, 4 September 2025

Unless otherwise stated, all content on this page was created by Jonas Michael-Lindhard, DTU Nanolab

Process runs
Date Substrate Information Process Information SEM Images
Wafer info Mask Material/ Exposed area Tool / Operator Conditioning Recipe Wafer ID Comments
2/12-2014 4" Wafer with travka50 mask AZ standard Si / 50+ % Pegasus/jmli 10 minute TDESC clean nanolab/jml/showerhead/prD/PrD01, 110 cyc or 6:14 mins S004691 New showerhead