Jump to content

Specific Process Knowledge/Etch/DRIE-Pegasus/showerheadchange: Difference between revisions

From LabAdviser
Jmli (talk | contribs)
No edit summary
Jmli (talk | contribs)
No edit summary
 
(70 intermediate revisions by the same user not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/DRIE-Pegasus/nanoetch click here]'''
<!--Checked for updates on 14/5-2018 - ok/jmli -->
<!-- Page reviewed 9/8-2022 jmli -->
<!--Checked for updates on 4/9-2025 - ok/jmli -->
= Modification of showerhead on Pegasus 1 in december 2014 =
{{Template:Author-jmli1}}
<!--Checked for updates on 2/02-2023 - ok/jmli -->
This page describes why the showerhead has been changed and what process changes have been found.
== Motivation ==
The showerhead that distributes the process gasses inside the Pegasus plasma source was changed. In the old design, the showerhead had a number of holes intended to distribute the gas uniformly inside the plasma source. The passage through the holes had a flow resistance that would cause the gasses coming from the MFC in a Bosch process to get mixed up - in this way working against the separation of the etch and dep cycles.
In the new design, the gas flow resistance has been reduced by increasing the diameter holes in the showerhead instead. This has no impact on processes that have a continuous gas flow - i.e. processes that are not switched. However, for processes with several gas flows that switch on and off, the switching from one gas flow to another will be much more well defined. This has enabled us to run Bosch processes with shorter cycles times. Shorter cycles times means smaller scallops and hence lower roughness and better control. We have not seen any changes to the uniformity of the plasma nor any other side effect. The modification was also done on Pegasus 2 and 3 before we started using them.
== Comparison of continuous processes on Pegasus 1==
=== Black silicon recipe ===
{| border="1" cellpadding="1" cellspacing="1" style="text-align:center;"
{| border="1" cellpadding="1" cellspacing="1" style="text-align:center;"
|+ '''Comparison of processes before and after the change of showerhead in December 2014'''
|-
|-
! colspan="2"| Process
! colspan="2"| Process
! colspan="3"| Before
! colspan="3"| Before (Old showerhead)
! colspan="3"| After
! colspan="3"| After (New showerhead)
|-
|-
! Name/Type
! Name/Type
! Description
! Description/parameters
! Wafer ID
! Wafer ID
! Comment
! Comment
Line 24: Line 45:
| [[file:S004679 centre.jpg |250px|frameless ]]
| [[file:S004679 centre.jpg |250px|frameless ]]
|-
|-
| S004592
| S003900
| Wafer edge
| Wafer edge
| [[file:S004592 edge.jpg |250px|frameless ]]
| [[file:S004592 edge.jpg |250px|frameless ]]
Line 31: Line 52:
| [[file:S004679 edge.jpg |250px|frameless ]]
| [[file:S004679 edge.jpg |250px|frameless ]]
|-
|-
! rowspan="2" width="100"| Switched etch of 1.8 µm polysilicon on BOX patterned with DUV
| rowspan="2" width="100"| 50 cycles, 30 degrees,  2.3/5 secs, 10/10 mtorr, 0/60 sccm SF<sub>6</sub>, 0/5 sccm O<sub>2</sub>, 50/20 sccm C<sub>4</sub>F<sub>8</sub>, 600/400 W coil, 0/40 W platen
| S004593
| 6" wafer
|[[file:S00459305.jpg|80px|frameless ]] [[file:S00459306.jpg|80px|frameless ]] [[file:S00459307.jpg|80px|frameless ]]


[[file:S00459308.jpg|80px|frameless ]] [[file:s004593-01.jpg|80px|frameless ]] [[file:s004593-02.jpg|80px|frameless ]]
|}
 
== Comparison of switched processes on Pegasus 1==
 
 
=== Process A ===


[[file:s004593-03.jpg|80px|frameless ]] [[file:s004593-04.jpg|80px|frameless ]]
{| border="1" cellpadding="1" cellspacing="0" style="text-align:center;"
| S004679
|-
| Wafer centre
! rowspan="2" width="100"| Recipe
| [[file:S004679 centre.jpg |250px|frameless ]]
! rowspan="2" width="20"| Name
! rowspan="2" width="20"| Temp.
! colspan="6" | Deposition step
! colspan="7" | Etch step
! colspan="3" | Comments
|-
! Time
! Pres.
! C<sub>4</sub>F<sub>8</sub>
! SF<sub>6</sub>
! O<sub>2</sub>
! Coil
! Time
! Pres.
! C<sub>4</sub>F<sub>8</sub>
! SF<sub>6</sub>
! O<sub>2</sub>
! Coil
! Platen
! Showerhead
! Runs
! width="100" | Key words
|-
! rowspan="4" | Process A    <!-- recipe name -->
! Step1 11 cyc <!-- step -->
| rowspan="2" |20      <!-- chiller temp -->
! 4      <!-- dep time -->
| 25      <!-- dep pressure -->
| 200      <!-- C4F8 flow -->
| 0      <!-- SF6 flow -->
| 0    <!-- O2 flow -->
| 2000      <!-- coil power -->
| 7.0      <!-- etch time -->
| 25(1.5s) 90>>150      <!-- etch pressure -->
| 0      <!-- C4F8 flow -->
| 350(1.5s) 550      <!-- SF6 flow -->
| 5      <!-- O2 flow -->
| 2800      <!-- coil power -->
| 120>>140(1.5s) 45      <!-- platen power -->
! rowspan="2" | Old      <!-- Showerhead -->
| rowspan="2" |[[Specific Process Knowledge/Etch/DRIE-Pegasus/showerheadchange/ProcessA | 1]]       <!-- link processes -->
| rowspan="2" |    <!-- keywords -->
|-
! Step2 44 cyc <!-- step -->
! 4      <!-- dep time -->
| 25      <!-- dep pressure -->
| 200      <!-- C4F8 flow -->
| 0      <!-- SF6 flow -->
| 0    <!-- O2 flow -->
| 2000      <!-- coil power -->
| 7.0      <!-- etch time -->
| 25(1.5s) 150      <!-- etch pressure -->
| 0      <!-- C4F8 flow -->
| 350(1.5s) 550      <!-- SF6 flow -->
| 5      <!-- O2 flow -->
| 2800      <!-- coil power -->
| 140(1.5s) 45      <!-- platen power -->
|-
! Step1 11 cyc <!-- step -->
| rowspan="2" |20      <!-- chiller temp -->
! 4      <!-- dep time -->
| 25      <!-- dep pressure -->
| 200      <!-- C4F8 flow -->
| 0      <!-- SF6 flow -->
| 0    <!-- O2 flow -->
| 2000      <!-- coil power -->
| 7.0      <!-- etch time -->
| 25(1.5s) 90>>150      <!-- etch pressure -->
| 0      <!-- C4F8 flow -->
| 350(1.5s) 550      <!-- SF6 flow -->
| 5      <!-- O2 flow -->
| 2800      <!-- coil power -->
| 120>>140(1.5s) 45      <!-- platen power -->
! rowspan="2" | New      <!-- Showerhead -->
| rowspan="2" |[[Specific Process Knowledge/Etch/DRIE-Pegasus/showerheadchange/ProcessA | 1]]       <!-- link processes -->
| rowspan="2" | Profile improved  <!-- keywords -->
|-
|-
| S004593
! Step2 44 cyc <!-- step -->
| Wafer edge
! 4      <!-- dep time -->
| [[file:S004592 edge.jpg |250px|frameless ]]
| 25      <!-- dep pressure -->
| S004679
| 200      <!-- C4F8 flow -->
| Wafer edge
| 0      <!-- SF6 flow -->
| [[file:S004679 edge.jpg |250px|frameless ]]
| 0    <!-- O2 flow -->
| 2000      <!-- coil power -->
| 7.0      <!-- etch time -->
| 25(1.5s) 150      <!-- etch pressure -->
| 0      <!-- C4F8 flow -->
| 350(1.5s) 550      <!-- SF6 flow -->
| 5      <!-- O2 flow -->
| 2800      <!-- coil power -->
| 140(1.5s) 45      <!-- platen power -->
|-
|-
|}
|}


=== SOI ===




{| border="1" cellpadding="1" cellspacing="0" style="text-align:center;"
|-
! rowspan="2" width="100"| Recipe
! rowspan="2" width="20"| Name
! rowspan="2" width="20"| Temp.
! colspan="6" | Deposition step
! colspan="7" | Etch step
! colspan="3" | Comments
|-
! Time
! Pres.
! C<sub>4</sub>F<sub>8</sub>
! SF<sub>6</sub>
! O<sub>2</sub>
! Coil
! Time
! Pres.
! C<sub>4</sub>F<sub>8</sub>
! SF<sub>6</sub>
! O<sub>2</sub>
! Coil
! Platen
! Showerhead
! Runs
! width="100" | Key words
|-
! rowspan="3" | SOI etch    <!-- recipe name -->
! SOI <!-- step -->
| 20      <!-- chiller temp -->
! 2      <!-- dep time -->
| 25      <!-- dep pressure -->
| 250      <!-- C4F8 flow -->
| 0      <!-- SF6 flow -->
| 0    <!-- O2 flow -->
| 2000      <!-- coil power -->
| 3      <!-- etch time -->
| 30      <!-- etch pressure -->
| 0      <!-- C4F8 flow -->
| 400      <!-- SF6 flow -->
| 40      <!-- O2 flow -->
| 2800      <!-- coil power -->
| 75 (0.025s, 75%)      <!-- platen power -->
! Old      <!-- Showerhead -->
| [[Specific Process Knowledge/Etch/DRIE-Pegasus/showerheadchange/SOI/SOI | 1]]      <!-- link processes -->
|  <!-- keywords -->
|-
! SOI <!-- step -->
| 20      <!-- chiller temp -->
! 2      <!-- dep time -->
| 25      <!-- dep pressure -->
| 250      <!-- C4F8 flow -->
| 0      <!-- SF6 flow -->
| 0    <!-- O2 flow -->
| 2000      <!-- coil power -->
| 3      <!-- etch time -->
| 30      <!-- etch pressure -->
| 0      <!-- C4F8 flow -->
| 400      <!-- SF6 flow -->
| 40      <!-- O2 flow -->
| 2800      <!-- coil power -->
| 75 (0.025s, 75%)      <!-- platen power -->
! New      <!-- Showerhead -->
| [[Specific Process Knowledge/Etch/DRIE-Pegasus/showerheadchange/SOI/SOI | 1]]      <!-- link processes -->
| OK  <!-- keywords -->
|-
|}
=== Process D ===




{| border="1" cellpadding="1" cellspacing="0" style="text-align:center;"
{| border="1" cellpadding="1" cellspacing="0" style="text-align:center;"
|+ '''Switched etch of 1.8 µm polysilicon on BOX patterned with DUV'''
|-
|-
! rowspan="2" width="100"| Recipe
! rowspan="2" width="100"| Recipe
! rowspan="2" width="20"| Step
! rowspan="2" width="20"| Name
! rowspan="2" width="20"| Temp.
! rowspan="2" width="20"| Temp.
! colspan="6" | Deposition step
! colspan="6" | Deposition step
! colspan="7" | Etch step
! colspan="7" | Etch step
! colspan="3" | Process observations
! colspan="3" | Comments
|-
|-
! Time
! Time
Line 79: Line 251:
! O<sub>2</sub>
! O<sub>2</sub>
! Coil  
! Coil  
| [[Main Page/Process Logs/jmli/Parameters#Platen power|Platen]]
! Platen
| [[Main Page/Process Logs/jmli/Parameters#Hardware | HW]]
! Showerhead
! Runs
! Runs
! width="100" | Key words
! width="100" | Key words
|-
|-
! -  <!-- recipe name -->
! rowspan="7" | Process D    <!-- recipe name -->
|        <!-- step -->
! Original <!-- step -->
|       <!-- chiller temp -->
| 0      <!-- chiller temp -->
|        <!-- dep time -->
! 2      <!-- dep time -->
|       <!-- dep pressure -->
| 20      <!-- dep pressure -->
|       <!-- C4F8 flow -->
| 150      <!-- C4F8 flow -->
|       <!-- SF6 flow -->
| 0      <!-- SF6 flow -->
|       <!-- O2 flow -->
| 0    <!-- O2 flow -->
|       <!-- coil power -->
| 2000      <!-- coil power -->
|       <!-- etch time -->
| 2.4      <!-- etch time -->
|       <!-- etch pressure -->
| 26      <!-- etch pressure -->
|       <!-- C4F8 flow -->
| 0      <!-- C4F8 flow -->
|       <!-- SF6 flow -->
| 275      <!-- SF6 flow -->
|       <!-- O2 flow -->
| 5      <!-- O2 flow -->
|       <!-- coil power -->
| 2500      <!-- coil power -->
|       <!-- platen power -->
| 35      <!-- platen power -->
|       <!-- hardware setting -->
! Old      <!-- Showerhead -->
|      <!-- link processes -->
| [[Specific Process Knowledge/Etch/DRIE-Pegasus/showerheadchange/ProcessD/original | 1]]      <!-- link processes -->
|     <!-- keywords -->
|   <!-- keywords -->
|-
! Original <!-- step -->
| 0      <!-- chiller temp -->
! 2      <!-- dep time -->
| 20      <!-- dep pressure -->
| 150      <!-- C4F8 flow -->
| 0     <!-- SF6 flow -->
| 0    <!-- O2 flow -->
| 2000      <!-- coil power -->
| 2.4      <!-- etch time -->
| 26      <!-- etch pressure -->
| 0      <!-- C4F8 flow -->
| 275      <!-- SF6 flow -->
| 5      <!-- O2 flow -->
| 2500      <!-- coil power -->
| 35      <!-- platen power -->
! New      <!-- Showerhead -->
| [[Specific Process Knowledge/Etch/DRIE-Pegasus/showerheadchange/ProcessD/original | 1]]      <!-- link processes -->
|   <!-- keywords -->
|-
|-
! base-A    <!-- recipe name -->
! New Process D <!-- step -->
| -      <!-- step -->
| 0       <!-- chiller temp -->
| 30       <!-- chiller temp -->
! 1       <!-- dep time -->
! 2.3       <!-- dep time -->
| 20       <!-- dep pressure -->
| 10       <!-- dep pressure -->
| 150       <!-- C4F8 flow -->
| 50       <!-- C4F8 flow -->
| 0      <!-- SF6 flow -->
| 0      <!-- SF6 flow -->
| 0    <!-- O2 flow -->
| 0    <!-- O2 flow -->
| 600       <!-- coil power -->
| 2000       <!-- coil power -->
| 5.0     <!-- etch time -->
! 3     <!-- etch time -->
| 10       <!-- etch pressure -->
| 26       <!-- etch pressure -->
| 20       <!-- C4F8 flow -->
| 0       <!-- C4F8 flow -->
| 60       <!-- SF6 flow -->
| 275       <!-- SF6 flow -->
| 5      <!-- O2 flow -->
| 5      <!-- O2 flow -->
| 400       <!-- coil power -->
| 2500       <!-- coil power -->
| 40     <!-- platen power -->
| 35     <!-- platen power -->
| -       <!-- hardware setting -->
! New       <!-- Showerhead -->
| [[Main Page/Process Logs/jmli/Pegasus/poly/base-A | 1]]      <!-- link processes -->
| [[Specific Process Knowledge/Etch/DRIE-Pegasus/showerheadchange/ProcessD/NewProcessD | 4]]      <!-- link processes -->
|   <!-- keywords -->
| Large undercut  <!-- keywords -->
|-
|-
! base-B    <!-- recipe name -->
! PrD01 <!-- step -->
| -      <!-- step -->
| 0       <!-- chiller temp -->
| 30       <!-- chiller temp -->
| 1       <!-- dep time -->
! 2.15       <!-- dep time -->
| 20       <!-- dep pressure -->
| 10       <!-- dep pressure -->
| 150       <!-- C4F8 flow -->
| 50       <!-- C4F8 flow -->
| 0      <!-- SF6 flow -->
| 0      <!-- SF6 flow -->
| 0    <!-- O2 flow -->
| 0    <!-- O2 flow -->
| 600       <!-- coil power -->
| 2000       <!-- coil power -->
| 5.0     <!-- etch time -->
! 2.4     <!-- etch time -->
| 10       <!-- etch pressure -->
| 26       <!-- etch pressure -->
| 20       <!-- C4F8 flow -->
| 0       <!-- C4F8 flow -->
| 60       <!-- SF6 flow -->
| 275       <!-- SF6 flow -->
| 5      <!-- O2 flow -->
| 5      <!-- O2 flow -->
| 400       <!-- coil power -->
| 2500       <!-- coil power -->
| 40     <!-- platen power -->
| 35     <!-- platen power -->
| -       <!-- hardware setting -->
| New       <!-- Showerhead -->
| [[Main Page/Process Logs/jmli/Pegasus/poly/base-B | 1]]      <!-- link processes -->
| [[Specific Process Knowledge/Etch/DRIE-Pegasus/showerheadchange/ProcessD/PrD01 | 2]]      <!-- link processes -->
|   <!-- keywords -->
|   <!-- keywords -->
|-
|-
! base-C    <!-- recipe name -->
! PrD02 <!-- step -->
| -      <!-- step -->
| 0       <!-- chiller temp -->
| 30       <!-- chiller temp -->
! 1.1       <!-- dep time -->
! 2.15       <!-- dep time -->
| 20       <!-- dep pressure -->
| 10       <!-- dep pressure -->
| 150       <!-- C4F8 flow -->
| 50       <!-- C4F8 flow -->
| 0      <!-- SF6 flow -->
| 0      <!-- SF6 flow -->
| 0    <!-- O2 flow -->
| 0    <!-- O2 flow -->
| 600       <!-- coil power -->
| 2000       <!-- coil power -->
| 5.0     <!-- etch time -->
| 2.4     <!-- etch time -->
| 10       <!-- etch pressure -->
| 26       <!-- etch pressure -->
| 20       <!-- C4F8 flow -->
| 0       <!-- C4F8 flow -->
| 60       <!-- SF6 flow -->
| 275       <!-- SF6 flow -->
| 5      <!-- O2 flow -->
| 5      <!-- O2 flow -->
| 400       <!-- coil power -->
| 2500       <!-- coil power -->
| 40     <!-- platen power -->
| 35     <!-- platen power -->
| -      <!-- hardware setting -->
| New      <!-- Showerhead -->
| [[Main Page/Process Logs/jmli/Pegasus/poly/base-B | 1]]      <!-- link processes -->
| [[Specific Process Knowledge/Etch/DRIE-Pegasus/showerheadchange/ProcessD/PrD02 | 1]]       <!-- link processes -->
|   <!-- keywords -->
|  <!-- keywords -->
|-
! PrD-3 <!-- step -->
| 0      <!-- chiller temp -->
| 1      <!-- dep time -->
| 20      <!-- dep pressure -->
| 150      <!-- C4F8 flow -->
| 0      <!-- SF6 flow -->
| 0    <!-- O2 flow -->
| 2000      <!-- coil power -->
! 2.5      <!-- etch time -->
| 26      <!-- etch pressure -->
| 0      <!-- C4F8 flow -->
| 275      <!-- SF6 flow -->
| 5      <!-- O2 flow -->
| 2500      <!-- coil power -->
| 35      <!-- platen power -->
| New      <!-- Showerhead -->
| [[Specific Process Knowledge/Etch/DRIE-Pegasus/showerheadchange/ProcessD/PrD-3 | 1]]      <!-- link processes -->
|  <!-- keywords -->
|-
! PrD-4 <!-- step -->
| 0      <!-- chiller temp -->
| 1      <!-- dep time -->
| 20      <!-- dep pressure -->
| 150      <!-- C4F8 flow -->
| 0      <!-- SF6 flow -->
| 0    <!-- O2 flow -->
| 2000      <!-- coil power -->
! 2.2      <!-- etch time -->
| 26      <!-- etch pressure -->
| 0      <!-- C4F8 flow -->
| 275      <!-- SF6 flow -->
| 5      <!-- O2 flow -->
| 2500      <!-- coil power -->
| 35      <!-- platen power -->
| New      <!-- Showerhead -->
| [[Specific Process Knowledge/Etch/DRIE-Pegasus/showerheadchange/ProcessD/PrD-4 | 1]]      <!-- link processes -->
| Best one so far!  <!-- keywords -->
|-
|-
|}
|}

Latest revision as of 09:32, 4 September 2025

Feedback to this page: click here


Modification of showerhead on Pegasus 1 in december 2014

Unless otherwise stated, all content on this page was created by Jonas Michael-Lindhard, DTU Nanolab

This page describes why the showerhead has been changed and what process changes have been found.

Motivation

The showerhead that distributes the process gasses inside the Pegasus plasma source was changed. In the old design, the showerhead had a number of holes intended to distribute the gas uniformly inside the plasma source. The passage through the holes had a flow resistance that would cause the gasses coming from the MFC in a Bosch process to get mixed up - in this way working against the separation of the etch and dep cycles.

In the new design, the gas flow resistance has been reduced by increasing the diameter holes in the showerhead instead. This has no impact on processes that have a continuous gas flow - i.e. processes that are not switched. However, for processes with several gas flows that switch on and off, the switching from one gas flow to another will be much more well defined. This has enabled us to run Bosch processes with shorter cycles times. Shorter cycles times means smaller scallops and hence lower roughness and better control. We have not seen any changes to the uniformity of the plasma nor any other side effect. The modification was also done on Pegasus 2 and 3 before we started using them.

Comparison of continuous processes on Pegasus 1

Black silicon recipe

Process Before (Old showerhead) After (New showerhead)
Name/Type Description/parameters Wafer ID Comment SEM images Wafer ID Comment SEM images
Continuous black silicon recipe on blank wafer 15 mins, -10 degrees, 32 mtorr, 60 sccm SF6, 55 sccm O2, 70 W platen S004592 Wafer centre S004679 Wafer centre
S003900 Wafer edge S004679 Wafer edge

Comparison of switched processes on Pegasus 1

Process A

Recipe Name Temp. Deposition step Etch step Comments
Time Pres. C4F8 SF6 O2 Coil Time Pres. C4F8 SF6 O2 Coil Platen Showerhead Runs Key words
Process A Step1 11 cyc 20 4 25 200 0 0 2000 7.0 25(1.5s) 90>>150 0 350(1.5s) 550 5 2800 120>>140(1.5s) 45 Old 1
Step2 44 cyc 4 25 200 0 0 2000 7.0 25(1.5s) 150 0 350(1.5s) 550 5 2800 140(1.5s) 45
Step1 11 cyc 20 4 25 200 0 0 2000 7.0 25(1.5s) 90>>150 0 350(1.5s) 550 5 2800 120>>140(1.5s) 45 New 1 Profile improved
Step2 44 cyc 4 25 200 0 0 2000 7.0 25(1.5s) 150 0 350(1.5s) 550 5 2800 140(1.5s) 45

SOI

Recipe Name Temp. Deposition step Etch step Comments
Time Pres. C4F8 SF6 O2 Coil Time Pres. C4F8 SF6 O2 Coil Platen Showerhead Runs Key words
SOI etch SOI 20 2 25 250 0 0 2000 3 30 0 400 40 2800 75 (0.025s, 75%) Old 1
SOI 20 2 25 250 0 0 2000 3 30 0 400 40 2800 75 (0.025s, 75%) New 1 OK

Process D

Recipe Name Temp. Deposition step Etch step Comments
Time Pres. C4F8 SF6 O2 Coil Time Pres. C4F8 SF6 O2 Coil Platen Showerhead Runs Key words
Process D Original 0 2 20 150 0 0 2000 2.4 26 0 275 5 2500 35 Old 1
Original 0 2 20 150 0 0 2000 2.4 26 0 275 5 2500 35 New 1
New Process D 0 1 20 150 0 0 2000 3 26 0 275 5 2500 35 New 4 Large undercut
PrD01 0 1 20 150 0 0 2000 2.4 26 0 275 5 2500 35 New 2
PrD02 0 1.1 20 150 0 0 2000 2.4 26 0 275 5 2500 35 New 1
PrD-3 0 1 20 150 0 0 2000 2.5 26 0 275 5 2500 35 New 1
PrD-4 0 1 20 150 0 0 2000 2.2 26 0 275 5 2500 35 New 1 Best one so far!