==Wet Silicon Nitride Etch==
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/Wet_Silicon_Nitride_Etch click here]'''
[[Image:Wet_nitride_etch.JPG|300x300px|thumb|Wet nitride etch: positioned in cleanroom 4]]
 
'''Unless anything else is stated, everything on this page, text and pictures are made by DTU Nanolab.'''
 
'''All links to Kemibrug (SDS) and Labmanager Including APV requires login.'''
 
'''All measurements on this page has been made by Nanolab staff.'''
 
 
 
[[index.php?title=Category:Equipment|Etch Wet silicon nitride]]
[[index.php?title=Category:Etch (Wet) bath|Silicon Nitride]]
 
[[Image:Nitrideetch.JPG|300x300px|thumb|The 'Nitride etch' bath is placed inside 'Wet bench 02: Nitride ethc' in Cleanroom D-3]]
 
 
Wet Etching of silicon nitride - stoichiometric and Si-rich - is done in a dedicated wetbench with an integrated quartz tank. The quartz tank can take up to 25 6" wafers in dedicated carriers. The 'Wetbench 02: Nitride etch' is placed in cleanroom D-3. The process is mainly used to strip silicon nitride (maskless), but can also be used for masked etching of silicon nitride using some kind of silicon oxide as etch mask. However, the wet silicon nitride etch is isotropic - meaning that the under-etching (etch-bias) at least amounts to the thickness of the silicon nitride layer.


Wet Etching of silicon nitride - stoichiometric and si-rich - is done in a dedicated laminar flow bench with an integrated quartz tank (Tiger Tank - TT-4). The quartz tank can take up to one 6" wafer carrier. The flow bench is placed in cleanroom 4. The process is mainly used to strip silicon nitride (maskless), but can also be used for masked etching of silicon nitride using some kind of silicon oxide as etch mask. However, the wet silicon nitride etch is isotropic meaning that the under-etching (etch-bias) at least amounts to the thickness of the silicon nitride layer.
The etch solution is initially 85 wt% H<sub>3</sub>PO<sub>4</sub> which is heated up to the boiling temperature - approx. 160°C.


The etch solution is initially 85 wt% H<sub>3</sub>PO<sub>4</sub> which is heated up to the boiling temperature - ca. 157 <sup>o</sup>C. Water is allowed to boil off thus raising the concentration and the boiling temperature of the solution until a boiling temperature of 180 <sup>o</sup>C is reached. Thereafter, the wafers are submerged into the bath and the water-cooled lid is closed to maintain the concentration and the boiling temperature. In some cases a lower boiling temperature is chosen - typically 160 <sup>o</sup>C - which lowers the etch rate and improves the selectivity R<sub>Si<sub>3</sub>N<sub>4</sub></sub> / R<sub>SiO<sub>2</sub></sub>.


'''NB: Great care has to be taken in this process due to risk of bumping. Therefore it is essential, that you stir thoroughly during heat up, before you start heating, at 50°C, 80°C and finally at 100°C'''


'''NB: Great care has to be taken in this process due to risk of "shock-boiling" '''


'''The user manual, user APV and contact information can be found in LabManager:'''
<!-- remember to remove the type of documents that are not present -->


[https://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=377 Nitride etch info page in LabManager],


===Nitride etch - key facts===
<br clear="all" />


{| border="1" cellspacing="0" cellpadding="4" align="left"
==Wet Silicon Nitride Etch==
!
 
! Nitride etch @ 180 <sup>o</sup>C
{|border="1" cellspacing="1" cellpadding="3" style="text-align:left;"  
! Nitride etch @ 160 <sup>o</sup>C
|-
|-
 
|General description
|-
|
|-style="background:silver; color:black"
Etch/strip of silicon nitride
!
|
! Nitride Etch @ 160<sup>o</sup>C
Etch/strip of silicon nitride
|-
|-
|Chemical solution
|H<sub>3</sub>PO<sub>4</sub>    (85 wt%)
|H<sub>3</sub>PO<sub>4</sub>    (85 wt%)


|-
|-
|Process temperature
|-style="background:WhiteSmoke; color:black"
|180 <sup>o</sup>C
!Generel description
|Etch/strip of silicon nitride
|-


|-
|-style="background:LightGrey; color:black"
!Link to safety APV and SDS
|[http://labmanager.danchip.dtu.dk/d4Show.php?id=1892&mach=130 see APV here]
[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhESk1OTEZKTVRkJWMyJTg3JTdjdiVjMiU4MyU3ZSVjMiU4OHYlYzIlODklN2UlYzIlODQlYzIlODMlYzIlODglNWVZUkk=#K see SDS here (requires login)]
|-
|-style="background:WhiteSmoke; color:black"
!Chemical solution
|H<sub>3</sub>PO<sub>4</sub>    (85 wt%)
|-
|-style="background:LightGrey; color:black"
!Process temperature
|160 <sup>o</sup>C
|160 <sup>o</sup>C
|-
|-
 
|-style="background:WhiteSmoke; color:black"
|Possible masking materials:
|'''Possible masking materials'''
|
|
*Thermal oxide (converted si-rich surface)
*Thermal oxide (converted si-rich surface)
*LPCVD-oxide (TEOS)
*LPCVD-oxide (TEOS)
*PECVD-oxide
*PECVD-oxide
|-
|-style="background:LightGrey; color:black"
!Etch rate
|
|
*Thermal oxide (converted si-rich surface)
*~26 Å/min (Si-rich Si<sub>3</sub>N<sub>4</sub>)
*LPCVD-oxide (TEOS)
*PECVD-oxide
|-
|-
|Etch rate
|-style="background:WhiteSmoke; color:black"
|
!Selectivity R<sub>Si<sub>3</sub>N<sub>4</sub></sub> / R<sub>SiO<sub>2</sub></sub>
*~85 Å/min (stoichiometric Si<sub>3</sub>N<sub>4</sub>)
|The selectivity (sirich nitride:oxide) is higher at 160 <sup>o</sup>C than at 180 <sup>o</sup>C
*~60 Å/min (si-rich Si<sub>3</sub>N<sub>4</sub>)
*~30 Å/min (annealed si-rich Si<sub>3</sub>N<sub>4</sub>)
*~4 Å/min (Thermal oxide)
|
*~?? Å/min (stoichiometric Si<sub>3</sub>N<sub>4</sub>)
*~26 Å/min (si-rich Si<sub>3</sub>N<sub>4</sub>)
*~4 Å/min (Thermal oxide)
|-
|-
|Batch size
|-style="background:LightGrey; color:black"
|
!Batch size
1-25 wafers at a time
|
|
1-25 wafer at a time
1-25 wafer at a time
|-
|-
|Size of substrate
|-style="background:WhiteSmoke; color:black"
!Size of substrate
|
|
2-6" wafers
2-6" wafers
|-
|-style="background:LightGrey; color:black"
!Allowed materials
|
|
2-6" wafers
*Silicon
*Silicon nitrides
*Silicon oxides
|-
|-
|}

Latest revision as of 09:14, 31 July 2025

Feedback to this page: click here

Unless anything else is stated, everything on this page, text and pictures are made by DTU Nanolab.

All links to Kemibrug (SDS) and Labmanager Including APV requires login.

All measurements on this page has been made by Nanolab staff.


Etch Wet silicon nitride Silicon Nitride

The 'Nitride etch' bath is placed inside 'Wet bench 02: Nitride ethc' in Cleanroom D-3


Wet Etching of silicon nitride - stoichiometric and Si-rich - is done in a dedicated wetbench with an integrated quartz tank. The quartz tank can take up to 25 6" wafers in dedicated carriers. The 'Wetbench 02: Nitride etch' is placed in cleanroom D-3. The process is mainly used to strip silicon nitride (maskless), but can also be used for masked etching of silicon nitride using some kind of silicon oxide as etch mask. However, the wet silicon nitride etch is isotropic - meaning that the under-etching (etch-bias) at least amounts to the thickness of the silicon nitride layer.

The etch solution is initially 85 wt% H3PO4 which is heated up to the boiling temperature - approx. 160°C.


NB: Great care has to be taken in this process due to risk of bumping. Therefore it is essential, that you stir thoroughly during heat up, before you start heating, at 50°C, 80°C and finally at 100°C


The user manual, user APV and contact information can be found in LabManager:

Nitride etch info page in LabManager,


Wet Silicon Nitride Etch

Nitride Etch @ 160oC
Generel description Etch/strip of silicon nitride
Link to safety APV and SDS see APV here

see SDS here (requires login)

Chemical solution H3PO4 (85 wt%)
Process temperature 160 oC
Possible masking materials
  • Thermal oxide (converted si-rich surface)
  • LPCVD-oxide (TEOS)
  • PECVD-oxide
Etch rate
  • ~26 Å/min (Si-rich Si3N4)
Selectivity RSi3N4 / RSiO2 The selectivity (sirich nitride:oxide) is higher at 160 oC than at 180 oC
Batch size

1-25 wafer at a time

Size of substrate

2-6" wafers

Allowed materials
  • Silicon
  • Silicon nitrides
  • Silicon oxides