Specific Process Knowledge/Thin film deposition/Deposition of Silver: Difference between revisions
Appearance
| (33 intermediate revisions by 5 users not shown) | |||
| Line 1: | Line 1: | ||
'''Feedback to this page''': '''[mailto: | '''Feedback to this page''': '''[mailto:LabAdviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Silver click here]''' | ||
<!-- Replace "http://labadviser. | <!-- Replace "http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin film deposition/Deposition of Aluminium" with the link to the Labadviser page--> | ||
<i> Unless otherwise stated, this page is written by <b>DTU Nanolab internal</b></i> | |||
<br clear="all" /> | <br clear="all" /> | ||
== Deposition of | == Deposition of silver == | ||
Silver can be deposited by e-beam evaporation, by sputtering and by thermal evaporation. In the chart below you can compare the different methods on the different deposition equipment. | Silver can be deposited by e-beam evaporation, by sputtering and by thermal evaporation. In the chart below you can compare the different methods on the different deposition equipment. | ||
== Sputter deposition of silver == | |||
* [[Specific Process Knowledge/Thin film deposition/Lesker |Sputter deposition of Silver in Lesker]]. | |||
== | == Thermal deposition of silver == | ||
* [[/Deposition of Silver in Thermal Evaporator|Thermal deposition of Silver in the Thermal Evaporator]] | |||
* [[/ | <br> | ||
<br> | |||
==Comparison of Deposition Equipment for Silver== | |||
{| border="1" cellspacing="0" cellpadding="4" | {| border="1" cellspacing="0" cellpadding="4" | ||
|-style="background:silver; color:black" | |-style="background:silver; color:black" | ||
! | ! | ||
! E-beam evaporation ([[Specific Process Knowledge/Thin film deposition/ | ! E-beam evaporation ([[Specific Process Knowledge/Thin film deposition/Temescal|E-beam evaporator (Temescal)]] and [[Specific Process Knowledge/Thin film deposition/10-pocket e-beam evaporator|E-beam evaporator (10-pockets)]]) | ||
! Thermal evaporation ([[Specific Process Knowledge/Thin film deposition/thermalevaporator|Thermal Evaporator]]) | |||
! | |||
! Sputter deposition ([[Specific Process Knowledge/Thin film deposition/Lesker|Lesker]]) | ! Sputter deposition ([[Specific Process Knowledge/Thin film deposition/Lesker|Lesker]]) | ||
! Sputter deposition ([[Specific Process Knowledge/Thin film deposition/Cluster-based multi-chamber high vacuum sputtering deposition system|Sputter-system Metal-Oxide (PC1) and Sputter-system Metal-Nitride (PC3)]]) | |||
|- | |- | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
! General description | ! General description | ||
| E-beam deposition of Ag | | E-beam deposition of Ag (line-of-sight, very good thickness uniformity) | ||
| Thermal deposition of Ag | | Thermal deposition of Ag (line-of-sight) | ||
| Sputter deposition of Ag (some step coverage) | |||
| Sputter deposition of Ag | | Sputter deposition of Ag including pulsed DC and HiPIMS | ||
| Sputter deposition of Ag | |||
|- | |- | ||
|-style="background:LightGrey; color:black" | |-style="background:LightGrey; color:black" | ||
! Pre-clean | ! Pre-clean | ||
| | | Ar ion etch (only in E-beam evaporator Temescal) | ||
| none | |||
| RF Ar clean | |||
| | | RF Ar clean | ||
|RF Ar clean | |||
|RF Ar clean | |||
|- | |- | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
| Line 58: | Line 48: | ||
! Layer thickness | ! Layer thickness | ||
|10Å to 1µm* | |10Å to 1µm* | ||
|10Å to 0.5µm | |10Å to 0.5µm ** | ||
|10Å to about 2000Å | |||
|10Å to ? | |||
|10Å to about | |||
|10Å to | |||
|- | |- | ||
|-style="background:LightGrey; color:black" | |-style="background:LightGrey; color:black" | ||
! Deposition rate | ! Deposition rate | ||
| | |1 to 10Å/s | ||
|5Å/s | |||
| | |Dependent on process parameters. | ||
|Dependent on | |||
|Dependent on process parameters. | |Dependent on process parameters. | ||
|- | |- | ||
| Line 78: | Line 64: | ||
! Batch size | ! Batch size | ||
| | | | ||
*Up to | *Up to 4x6" wafers or | ||
*Up to 3x8" wafers | |||
or | |||
*smaller pieces | *smaller pieces | ||
| | | | ||
* | *Up to 1x8" wafer or 1x6" wafer | ||
*Up to 3x4" wafers | |||
*smaller pieces | |||
* | |||
* | |||
| | | | ||
*1x6" wafers or | *1x6" wafers or | ||
*1x4" wafers or | *1x4" wafers or | ||
*smaller pieces | *smaller pieces | ||
| | |||
*up to 10x6" wafers or | |||
*up to 10x4" wafers or | |||
*many smaller pieces | |||
|-style="background:Lightgrey; color:black" | |-style="background:Lightgrey; color:black" | ||
!Allowed materials | !Allowed materials | ||
| | | | ||
* | *Almost any as long as it does not outgas if you plan to use substrate heating. See cross-contamination sheets in Labmanager. | ||
| | | | ||
* | *Almost any as long as it does not outgas. See cross-contamination sheet in Labmanager. | ||
| | | | ||
* | * Almost any that do not degas. See also the [https://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=244 cross-contamination sheet] | ||
| | | | ||
* | *Almost any that does not degas at your intended substrate temperature. See cross contamination sheets for [https://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=441 PC1] and [https://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=442 PC3] | ||
|-style="background:whitesmoke; color:black" | |-style="background:whitesmoke; color:black" | ||
! Comment | ! Comment | ||
| | | Pumpdown approx 20 min. Possible to tilt the wafer to achieve tunable step coverage. | ||
| Pumpdown approx 15 min. | |||
|Load and transfer < 10 minutes | |||
| | |Load and transfer approx. 12 minutes | ||
| | |||
| | |||
|- | |- | ||
|} | |} | ||
'''*''' ''For thicknesses above 200 nm permission | '''*''' ''For thicknesses above 600 nm please get permission from ThinFilm group by writing to metal@nanolab.dtu.dk'' | ||
'''**''' ''For thicknesses above 200 nm please get permission from ThinFilm group by writing to metal@nanolab.dtu.dk'' | |||