mrEBL6000 works as a negative e-beam resist but is also UV sensitive, why resist and coated wafers should be kept in yellow rooms only. When carrying the wafers to the e-beam writer, use a black or blue box for protection. While mounting the wafers in the e-beam cassettes, you can turn off the white light in the e-beam room and turn on the yellow light which is located above the pre-aligner setup. Please mount as close to exposure as possible and turn of the with light outside the room and place a note on the door not to turn on light while the cassette is in the stocker. | |||
mrEBL6000 is a chemically amplified resist, i.e. immediately after e-beam exposure, the wafers require a post-exposure bake. If no post-exposure bake is performed, the resist is not crosslinked and will most likely dissolve during development. | |||
This resist can be used as standard negative resist at Nanolab, but due to limited use, we often need to buy a new bottle, hence please ask long time (up to 3 months) in advance for this chemical. or by it yourself! | |||
<br> | |||
<br> | |||
<br> | |||
== 3 week project on mrEBL6000 by William Tiddi == | |||
mrEBL6000 was studied April 2015 by William Tiddi; the report can be found [[media:Report (2).pdf|here]]. | |||
<br> | |||
<br> | |||
== Spin Curve == | |||
[[File:image001.png|right|600px]] | |||
| | |||
The thickness is measured on VASE Ellipsometer using a simple Cauchy model for a transparent polymer on Si. The measurements are performed at one incidence angle (70 degrees) only. | |||
9 points on each 4" wafer has been measured; the standard deviation thus representing the homogeinity of the film on the 4" wafers. | |||
| | {|border="1" cellspacing="0" cellpadding="3" style="text-align:left;" style="width: 30%" | ||
|- | |- | ||
|- | |- | ||
|-style="background: | |-style="background:#0048BA; color:White" | ||
!colspan=" | !colspan="3"|MicroResist mr EBL 6000. Spin coated on Spin Coater: Manual LabSpin A-5, WILTID, 2015. Softbake 3 min @ 110 degC. | ||
|- | |- | ||
|- | |- | ||
|-style="background: | |-style="background:WhiteSmoke; color:black" | ||
!Spin Speed [rpm] | |||
!Thickness [nm] | |||
!St Dev | |||
|- | |- | ||
|- | |- | ||
|-style="background:WhiteSmoke; color:black | |-style="background:WhiteSmoke; color:black" | ||
|2000 | |||
|103 | |||
|0.5 | |||
|- | |- | ||
|- | |- | ||
|-style="background: | |-style="background:WhiteSmoke; color:black" | ||
| | |3000 | ||
| | |88 | ||
|0.4 | |||
| | |||
|- | |- | ||
|- | |- | ||
|-style="background:WhiteSmoke; color:black | |-style="background:WhiteSmoke; color:black" | ||
|4000 | |||
|78 | |||
|0.4 | |||
|- | |- | ||
|- | |- | ||
|-style="background: | |-style="background:WhiteSmoke; color:black" | ||
| | |5000 | ||
| | |71 | ||
|0.7 | |||
| | |||
|- | |- | ||
|- | |- | ||
|-style="background: | |-style="background:WhiteSmoker; color:black" | ||
|6000 | |||
|68 | |||
|0.5 | |||
|- | |- | ||
|- | |- | ||
|-style="background: | |-style="background:WhiteSmoker; color:black" | ||
| | |7000 | ||
| | |66 | ||
| | |0.6 | ||
|- | |- | ||
|} | |} | ||
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;" style="width: 30%" | |||
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;" style="width: | |||
|- | |- | ||
|- | |- | ||
|-style="background: | |-style="background:#E30022; color:White" | ||
!colspan=" | !colspan="3"|MicroResist mr EBL 6000 diluted 1:1 in anisole. Spin coated on Spin Coater: Manual LabSpin A-5, WILTID, 2015. Softbake 3 min @ 110 degC. | ||
|- | |- | ||
| Line 146: | Line 101: | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
!Spin Speed [rpm] | !Spin Speed [rpm] | ||
!Thickness [nm] | !Thickness [nm] | ||
!St Dev | !St Dev | ||
| Line 154: | Line 108: | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
|2000 | |2000 | ||
| | |50 | ||
|0.2 | |||
|0. | |||
|- | |- | ||
| Line 162: | Line 115: | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
|3000 | |3000 | ||
| | |42 | ||
|0.5 | |||
|0. | |||
|- | |- | ||
| Line 170: | Line 122: | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
|4000 | |4000 | ||
| | |38 | ||
|0.5 | |0.5 | ||
|- | |- | ||
| Line 178: | Line 129: | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
|5000 | |5000 | ||
| | |34 | ||
|0.3 | |||
|0. | |||
|- | |- | ||
| Line 186: | Line 136: | ||
|-style="background:WhiteSmoker; color:black" | |-style="background:WhiteSmoker; color:black" | ||
|6000 | |6000 | ||
| | |32 | ||
|0.3 | |||
|0. | |||
|- | |- | ||
|- | |||
|-style="background:WhiteSmoker; color:black" | |||
|7000 | |||
|32 | |||
|0.3 | |||
|- | |||
|} | |} | ||
<br> | |||
<br> | |||
==Contrast Curve== | |||
The contrast curve is measured on lines 100 nm in width, exposed with doses in the range of 6-63 µC/cm2. After exposure, the sample has been post-exposure baked 5 min @ 110 degree C. Development is performed with mr-DEV 600 in 40s followed by an IPA rinse 60s. | |||
These measurements are performed by WILTID April 2015. | |||