Specific Process Knowledge/Thin film deposition/Deposition of NiV: Difference between revisions

From LabAdviser
Knil (talk | contribs)
No edit summary
Reet (talk | contribs)
 
(18 intermediate revisions by 4 users not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php?title=Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_NiV click here]'''
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php?title=Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_NiV click here]'''


Nickel Vanadium can be deposited by sputter evaporation. In the chart below you can compare the different deposition equipment.
==Sputtering of Nickel Vanadium==


Nickel Vanadium may be sputter deposited in either Sputter-system (Lesker) or Wordentec. The following pages show both process parameters and data on surface roughness of the deposited films
* [[/Sputtering of NiV in Lesker|Sputtering of NiV in Lesker]]
* [[/Sputtering of NiV in Sputter-System Metal-Oxide (PC1)|Sputtering of NiV in Sputter-System Metal-Oxide (PC1)]]
* [[/Sputtering of NiV in Wordentec|Sputtering of NiV in Wordentec]]
In the chart below you can compare the different deposition equipment.


{| border="1" cellspacing="0" cellpadding="4"  
{| border="1" cellspacing="0" cellpadding="4"  
Line 8: Line 16:
!  
!  


! Sputter deposition ([[Specific Process Knowledge/Thin film deposition/Multisource PVD|PVD co-sputter/evaporation]])
|Sputter deposition ([[Specific Process Knowledge/Thin film deposition/Lesker|Sputter-System Lesker]])
! Sputter deposition ([[Specific Process Knowledge/Thin film deposition/Lesker|Sputter-System Lesker]])
|Sputter deposition ([[Specific Process Knowledge/Thin film deposition/Cluster-based multi-chamber high vacuum sputtering deposition system|Sputter-system Metal-Oxide (PC1) and Sputter-system Metal-Nitride (PC3)]])
|Sputter deposition ([[Specific Process Knowledge/Thin film deposition/Wordentec|Wordentec]])
|-  
|-  
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
! Batch size
! General description
| Sputter deposition of NiV
| Sputter deposition of NiV
| Sputter deposition of NiV
|-


|
*12x2" wafers or
*12x4" wafers or
*4x6" wafers
|
*Pieces or
*1x4" wafer or
*1x6" wafer
|-
|-style="background:LightGrey; color:black"
|-style="background:LightGrey; color:black"
! Pre-clean
! Pre-clean
Line 28: Line 33:
|RF Ar clean
|RF Ar clean
|RF Ar clean
|RF Ar clean
| none
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
! Layer thickness
! Layer thickness


|About 10Å to 4000Å
|About 10Å to 5000Å
|About 10Å to 5000Å
|About 10Å to 5000Å
|About 10Å to 5000Å
|-
|-
|-style="background:LightGrey; color:black"
|-style="background:LightGrey; color:black"
! Deposition rate
! Deposition rate


|Depending on process parameters.
|Depending on process parameters(normally less than 1 A/sec).
|Depending on process parameters.
|Depending on process parameters(normally less than 1 A/sec).
|Depending on process parameters(normally less than 1 A/sec).
 
|-
 
|-style="background:WhiteSmoke; color:black"
! Batch size
 
|
*Pieces or
*1x4" wafer or
*1x6" wafer
 
|
*Up to 10x4" or 6" wafers
*Many smaller pieces
|
*24x2" wafers or
*6x4" wafers or
*6x6" wafers
|-


|-style="background:LightGrey; color:black"
! Allowed substrates
|
* Silicon wafers
* Quartz wafers
* Pyrex wafers(No substrate heating)
|
* Almost any that do not outgas.
|
* Silicon wafers
* Quartz wafers
* Pyrex wafers
|-
|-
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
!Allowed materials
!Allowed materials


|
|
* Silicon
* Silicon oxide  
* Silicon oxide  
* Silicon nitride
* Silicon (oxy)nitride  
* Silicon (oxy)nitride  
* Photoresist  
* Photoresist  
Line 52: Line 97:
* SU-8  
* SU-8  
* Metals  
* Metals  
* Carbon
|
* Almost any that do not outgas.
|
|
* Silicon
* Silicon
Line 62: Line 110:
* SU-8  
* SU-8  
* Metals  
* Metals  
* Carbon
* Carbon  
 


|-style="background:LightGrey; color:black"
|-style="background:LightGrey; color:black"
! Target size
| 2 inch sputter target
| 3 inch sputter target
(or in special cases 4 inch)
| 6 inch sputter target
|-
|-style="background:WhiteSmoke; color:black"
! Comment
! Comment


| Sputter target with NiV composition: Ni/V 93/7%  
|  
| Sputter target with NiV composition: Ni/V 93/7%
*Sputter target with NiV composition: Ni/V 93/7%
*Substrate rotation
*Substrate RF Bias (optional)
|  
*Sputter target with NiV composition: Ni/V 93/7%
*Substrate rotation
*Substrate RF Bias (optional)
|
*Sputter target with NiV composition: Ni/V 93/7%
*No substrate rotation
*No substrate RF Bias
 
|-
|-
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"

Latest revision as of 09:27, 9 June 2023

Feedback to this page: click here

Sputtering of Nickel Vanadium

Nickel Vanadium may be sputter deposited in either Sputter-system (Lesker) or Wordentec. The following pages show both process parameters and data on surface roughness of the deposited films


In the chart below you can compare the different deposition equipment.

Sputter deposition (Sputter-System Lesker) Sputter deposition (Sputter-system Metal-Oxide (PC1) and Sputter-system Metal-Nitride (PC3)) Sputter deposition (Wordentec)
General description Sputter deposition of NiV Sputter deposition of NiV Sputter deposition of NiV
Pre-clean RF Ar clean RF Ar clean none
Layer thickness About 10Å to 5000Å About 10Å to 5000Å About 10Å to 5000Å
Deposition rate Depending on process parameters(normally less than 1 A/sec). Depending on process parameters(normally less than 1 A/sec). Depending on process parameters(normally less than 1 A/sec).
Batch size
  • Pieces or
  • 1x4" wafer or
  • 1x6" wafer
  • Up to 10x4" or 6" wafers
  • Many smaller pieces
  • 24x2" wafers or
  • 6x4" wafers or
  • 6x6" wafers
Allowed substrates
  • Silicon wafers
  • Quartz wafers
  • Pyrex wafers(No substrate heating)
  • Almost any that do not outgas.
  • Silicon wafers
  • Quartz wafers
  • Pyrex wafers
Allowed materials
  • Silicon
  • Silicon oxide
  • Silicon nitride
  • Silicon (oxy)nitride
  • Photoresist
  • PMMA
  • Mylar
  • SU-8
  • Metals
  • Carbon
  • Almost any that do not outgas.
  • Silicon
  • Silicon oxide
  • Silicon nitride
  • Silicon (oxy)nitride
  • Photoresist
  • PMMA
  • Mylar
  • SU-8
  • Metals
  • Carbon


Target size 2 inch sputter target 3 inch sputter target

(or in special cases 4 inch)

6 inch sputter target


Comment
  • Sputter target with NiV composition: Ni/V 93/7%
  • Substrate rotation
  • Substrate RF Bias (optional)
  • Sputter target with NiV composition: Ni/V 93/7%
  • Substrate rotation
  • Substrate RF Bias (optional)
  • Sputter target with NiV composition: Ni/V 93/7%
  • No substrate rotation
  • No substrate RF Bias