== Cleaning of wafers == | |||
__NOTOC__ | |||
During processing it is sometimes mandatory, necessary or just recommended to clean the wafers or the photo lithographic masks. This can be done by different cleaning procedures depending on what the wafers have been exposed to, and where they are going to be further processed. In the comparison table below is listed different cleaning procedures available at nanolab. | |||
===Wafers that go into the high temperature furnaces=== | |||
As a general rule all wafers that go into the high temperature furnaces need a full RCA clean directly before the furnace step. | |||
There are, however, some exception to this rule. Please find more information on wafer cleaning before furnace processes [https://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Thermal_Process/Storage_and_cleaning_of_wafer_to_the_A,_B,_C_and_E_stack_furnaces here]. | |||
<br/> | |||
<br/> | |||
===Wafers that have been in KOH baths (Si Etch 1, 2 and 3), KOH BHF baths or 'Nitride etch: H3PO4' (warm phosphoric acid)=== | |||
Wafers that have been etched in KOH are often etched in warm phosphoric acid afterwards to strip the silicon nitride etch mask. Therefore, wafers that have been processed in KOH baths, KOH BHF baths or phosphoric acid nitride etch baths often need at minimum a 7-up or Piranha clean before they can be further processed (in order to remove KOH etch residuals and metal ions). | |||
<br/> | |||
<br/> | |||
== | ===Items that have been outside the cleanroom=== | ||
Before bringing samples into the cleanroom you have to get approval from Nanolab ("Bring samples into cleanroom"-procedure). The approval process and cleaning procedure is described on <b>[[Specific_Process_Knowledge/Wafer_cleaning/Bring_samples_into_Cleanroom_or_PolyFabLab| here]]</b>. Please note that the approval for bringing samples into the cleanroom is personal (and fellow group members need to send in seperate request). | |||
<br/> | |||
<br/> | |||
===Masks=== | |||
Masks that have become dirty by dust particles or resist residues have to be cleaned in the 7-up (mask) bath before use. You can find more information [https://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Wafer_cleaning/7-up_%26_Piranha here]. | |||
<br/> | |||
<br/> | |||
== | ===Before entering specific process equipment=== | ||
Sometimes the wafers need a certain cleaning process before they can enter specific process equipments due to the risk of cross contamination. Please consult the cross contamination scheme to see whether your wafers need a cleaning before the next processing sequence. <br \> | |||
<br/> | |||
<br/> | |||
==Comparison of Wafer Cleaning Methods== | ==Comparison of Wafer Cleaning Methods== | ||
| Line 16: | Line 39: | ||
! | ! | ||
![[Specific Process Knowledge/Wafer cleaning/RCA|RCA]] | ![[Specific Process Knowledge/Wafer cleaning/RCA|RCA]] | ||
![[Specific Process Knowledge/Wafer cleaning/7-up & Piranha| | ![[Specific Process Knowledge/Wafer cleaning/7-up & Piranha|Wafer/Mask Clean baths & Piranha]] | ||
![[Specific Process Knowledge/Wafer cleaning/cleaning with HF|5% HF]] | ![[Specific Process Knowledge/Wafer cleaning/cleaning with HF|5% HF]] | ||
![[Specific Process Knowledge/Wafer cleaning/IMEC|IMEC]] | ![[Specific Process Knowledge/Wafer cleaning/IMEC|IMEC]] | ||
![[Specific Process Knowledge/Wafer cleaning/Cleaning with Soap Sonic|Soap Sonic]] | ![[Specific Process Knowledge/Wafer cleaning/Cleaning with Soap Sonic|Soap Sonic]] | ||
![[Specific Process Knowledge/Wafer cleaning/Post CMP Cleaner|Post CMP Cleaner]] | |||
|- | |- | ||
| Line 25: | Line 49: | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
!Generel description | !Generel description | ||
|Two step process to remove organics and metals | |Two step process to remove traces of organics and metals | ||
|Removes organics and alkali ions | |Removes traces of organics and alkali ions | ||
|Removing native oxide | |Removing native oxide | ||
| | |Removing dust, traces of organics and alkali ions and slightly polish the surface. | ||
Make the surface hydrophillic | |||
|Removing dust and particles | |Removing dust and particles | ||
|Removing slurry residues from the CMP | |||
|- | |- | ||
| Line 40: | Line 66: | ||
|Recommended cleaning and treatment before wafer bonding | |Recommended cleaning and treatment before wafer bonding | ||
|Mandatory cleaning of very dirty items that enters the cleanroom. Should always be followed by a piranha clean. | |Mandatory cleaning of very dirty items that enters the cleanroom. Should always be followed by a piranha clean. | ||
|Recommended cleaning after CMP | |||
|- | |- | ||
| Line 56: | Line 83: | ||
| | | | ||
*All sizes that can go into the bath | *All sizes that can go into the bath | ||
| | |||
*<nowiki>#</nowiki>1 20x20mm sample as well as 2", 4" and 6inch wafers | |||
|- | |- | ||
| Line 75: | Line 104: | ||
*Silicon Oxynitride | *Silicon Oxynitride | ||
*Quartz/fused silica | *Quartz/fused silica | ||
*Pyrex and wafers with Cr ONLY in Mask | *Pyrex, other glass and Silicon wafers with Cr ONLY allowed in Mask Cleaning bath or beaker in fumehood | ||
| | | | ||
*Silicon | *Silicon | ||
| Line 95: | Line 124: | ||
| | | | ||
*All materials | *All materials | ||
| | |||
*Silicon | |||
*Poly Silicon | |||
*Silicon Oxide | |||
*Quartz/fused silica | |||
|- | |- | ||
|} | |} | ||
Latest revision as of 15:51, 25 September 2026
Cleaning of wafers
During processing it is sometimes mandatory, necessary or just recommended to clean the wafers or the photo lithographic masks. This can be done by different cleaning procedures depending on what the wafers have been exposed to, and where they are going to be further processed. In the comparison table below is listed different cleaning procedures available at nanolab.
Wafers that go into the high temperature furnaces
As a general rule all wafers that go into the high temperature furnaces need a full RCA clean directly before the furnace step.
There are, however, some exception to this rule. Please find more information on wafer cleaning before furnace processes here.
Wafers that have been in KOH baths (Si Etch 1, 2 and 3), KOH BHF baths or 'Nitride etch: H3PO4' (warm phosphoric acid)
Wafers that have been etched in KOH are often etched in warm phosphoric acid afterwards to strip the silicon nitride etch mask. Therefore, wafers that have been processed in KOH baths, KOH BHF baths or phosphoric acid nitride etch baths often need at minimum a 7-up or Piranha clean before they can be further processed (in order to remove KOH etch residuals and metal ions).
Items that have been outside the cleanroom
Before bringing samples into the cleanroom you have to get approval from Nanolab ("Bring samples into cleanroom"-procedure). The approval process and cleaning procedure is described on here. Please note that the approval for bringing samples into the cleanroom is personal (and fellow group members need to send in seperate request).
Masks
Masks that have become dirty by dust particles or resist residues have to be cleaned in the 7-up (mask) bath before use. You can find more information here.
Before entering specific process equipment
Sometimes the wafers need a certain cleaning process before they can enter specific process equipments due to the risk of cross contamination. Please consult the cross contamination scheme to see whether your wafers need a cleaning before the next processing sequence.
Comparison of Wafer Cleaning Methods
| RCA | Wafer/Mask Clean baths & Piranha | 5% HF | IMEC | Soap Sonic | Post CMP Cleaner | |
|---|---|---|---|---|---|---|
| Generel description | Two step process to remove traces of organics and metals | Removes traces of organics and alkali ions | Removing native oxide | Removing dust, traces of organics and alkali ions and slightly polish the surface.
Make the surface hydrophillic |
Removing dust and particles | Removing slurry residues from the CMP |
| Purpose | Mandatory prior furnace processes | When needed and always after KOH etch and Nitride etch in Phosphoric acid. Sometimes mandatory before next processing step. | Optional during RCA cleaning | Recommended cleaning and treatment before wafer bonding | Mandatory cleaning of very dirty items that enters the cleanroom. Should always be followed by a piranha clean. | Recommended cleaning after CMP |
| Substrate size |
|
|
|
|
|
|
| Allowed materials |
|
|
|
|
|
|