Jump to content

Specific Process Knowledge/Etch/Wet Silicon Oxide Etch (BHF): Difference between revisions

From LabAdviser
Kabi (talk | contribs)
Hvje (talk | contribs)
 
(79 intermediate revisions by 9 users not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:wetchemistry@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Etch/Wet_Silicon_Oxide_Etch_(BHF) click here]'''
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/Wet_Silicon_Oxide_Etch_(BHF) click here]'''


'''''Unless anything else is stated, everything on this page, text and pictures are made by DTU Nanolab.'''''


==Wet Silicon Oxide Etch (BHF, HF and SIO Etch (wetting agent))==
'''''All links to Kemibrug (SDS) and Labmanager Including APV, requires login.'''''


Silicon oxide can be etched using HF. At Danchip it is mainly used in a buffered version BHF (premixed). You can find the KBA [http://kemibrug.dk/KBA/CAS/106534/?show_KBA=1&portaldesign=1 here] The BHF has a more stable etch rate and is more gentle to photoresist due to an almost pH neutral solution which makes photoresist a good masking material for the oxide etch.
[[index.php?title=Category:Equipment|Etch Wet Silicon Oxide]]
[[index.php?title=Category:Etch (Wet) bath|Silicon Oxide]]


SIO etch (BHF with wetting agent) can also be used for etching silicon oxide. This is mainly for etching small holes. If you have wetting problems in BHF try the SIO etch. It is also a good idea to wet the sample in water for a few minutes before etching.
==Wet Silicon Oxide Etch (BHF, HF and BOE 7:1 Etchant VLSI)==


Wafers with metals or other materials, not allowed in the dedicated oxide etch baths, can be etched in the PP-bath positioned in the fume hood in cleanroom 2 or in a '''plastic''' beaker.  
Silicon oxide can be etched using HF. At DTU Nanolab it is mainly used in a buffered version BHF (premixed). You can find safety datasheets on Kemibrug [http://kemibrug.dk here] The BHF has a stable etch rate and is gentle to photoresist due to an almost pH neutral solution which makes photoresist a good masking material for the oxide etch.
 
BOE 7:1 Etchant VLSI with Surfactant (BHF with wetting agent) can also be used for etching silicon oxide. This is mainly for etching small holes. At DTU Nanolab we do not have BHF with wetting agent in a prepared bath, it's only to be used in fumehoods. It's not very often used and we do not have it as a standard chemical. Please contact DTU Nanolab if you need it. 
 
Wafers with metals or other materials, not allowed in the dedicated oxide etch baths, can be etched using a '''plastic beaker''' in Fume hood 01 or 02 (Acids/bases) in D-3. Samples with III-V materials (e.g. InP and GaAs) must be etched in Fume hood 07: III-V Avids/bases in D-3.
<br>
 
'''The user manual for Oxide etch 1: BHF, APV's and contact information can be found in LabManager''' [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=389 by clicking here]
 
'''The user manual for Oxide etch 2: BHF (clean), APV's and contact information can be found in LabManager''' [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=378 by clicking here]
 
'''The user manual for Oxide etch 3: 10% HF, APV's and contact information can be found in LabManager''' [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=380 by clicking here]
 
'''The user manual for various HF baths in RCA and Fume hoods, APV's and contact information can be found in LabManager''' [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=64 by clicking here]
 
'''<big>Working with HF above 13% is only allowed by Nanolab staff</big>'''


'''The user manual for all HF/BHF baths, APV's and contact information can be found in LabManager:'''[http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=64 by clicking here]
<!-- remember to remove the type of documents that are not present -->
<!-- remember to remove the type of documents that are not present -->
'''Process information:''' <br>
See more [[/BHF etch rates|etch rates]] in HF solutions.




Line 18: Line 38:
!colspan="2" border="none" style="background:silver; color:black;" align="center"|Etchant  
!colspan="2" border="none" style="background:silver; color:black;" align="center"|Etchant  
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Etch/Wet_Silicon_Oxide_Etch_(BHF)#Comparing_different_BHF_baths|BHF]]</b>
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Etch/Wet_Silicon_Oxide_Etch_(BHF)#Comparing_different_BHF_baths|BHF]]</b>
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Etch/Wet_Silicon_Oxide_Etch_(BHF)#Comparing_different_5.25_HF_baths|5% HF]]</b>
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Etch/Wet_Silicon_Oxide_Etch_(BHF)#Comparing_different_5.25_HF_baths|1% HF / 5% HF / 10% HF]]</b>
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Etch/Wet_Silicon_Oxide_Etch_(BHF)#Comparing_different_40.25_HF_baths|40% HF]]</b>
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Etch/Wet_Silicon_Oxide_Etch_(BHF)#Comparing_different_40.25_HF_baths|40% HF]]</b>
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Etch/Wet_Silicon_Oxide_Etch_(BHF)#SiO_etch_bath|SiO etch]]</b>
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Etch/Wet_Silicon_Oxide_Etch_(BHF)#SiO_etch_bath|BOE 7:1 Etchant VLSI with Surfactant]]</b>
|-
|-
!style="background:silver; color:black;" align="center" width="60" rowspan="2"|Purpose  
!style="background:silver; color:black;" align="center" width="60" rowspan="2"|Purpose  
Line 29: Line 49:
*Mainly for removing native oxide
*Mainly for removing native oxide
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Mainly for etching deep into borofloat or quartz wafers
*Mainly for etching deep into borofloat or quartz wafers. '''Only Nanolab staff are allowed to work with this HF'''.
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Etching of silicon oxide - especially for etching small holes
*Etching of silicon oxide - especially for etching small holes
|-
|-
|style="background:LightGrey; color:black"|Link to safety APV and KBA
|style="background:LightGrey; color:black"|Link to safety APV and SDS (You must be logged in to Kemibrug to view SDSs)
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*:[http://labmanager.danchip.dtu.dk/d4Show.php?id=1897&mach=64 see APV here]
*:[http://labmanager.nanolab.dtu.dk/d4Show.php?id=1897&mach=64 see APV here]
*:[http://kemibrug.dk/KBA/CAS/106534/?show_KBA=1&portaldesign=1 see KBA here]
*:[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhESkhKSUxMVGQlYzIlODclN2N2JWMyJTgzJTdlJWMyJTg4diVjMiU4OSU3ZSVjMiU4NCVjMiU4MyVjMiU4OCU1ZVlSSQ==#K see SDS here]
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*:[http://labmanager.danchip.dtu.dk/d4Show.php?id=1897&mach=64 see APV here]
*:[http://labmanager.danchip.dtu.dk/d4Show.php?id=1897&mach=64 see APV here]
*:[http://kemibrug.dk/KBA/CAS/106231/?show_KBA=1&portaldesign=1 see KBA here]
*:[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhERkZMSkhFR1RkJWMyJTg3JTdjdiVjMiU4MyU3ZSVjMiU4OHYlYzIlODklN2UlYzIlODQlYzIlODMlYzIlODglNWVZUkk=#K see SDS here]
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*:[http://labmanager.danchip.dtu.dk/d4Show.php?id=2479&mach=146 see APV here]
*:[http://labmanager.danchip.dtu.dk/d4Show.php?id=2479&mach=146 see APV here]
*:[http://kemibrug.dk/KBA/CAS/100648/?lang=da&show_KBA=1&portaldesign=1 see KBA here]
*:[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhERkZMSkhOSVRkJWMyJTg3JTdjdiVjMiU4MyU3ZSVjMiU4OHYlYzIlODklN2UlYzIlODQlYzIlODMlYzIlODglNWVZUkk=#K see SDS here]
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*:[http://labmanager.danchip.dtu.dk/d4Show.php?id=1897&mach=64 see APV here]
*:[http://labmanager.danchip.dtu.dk/d4Show.php?id=1897&mach=64 see APV here]
*:[http://kemibrug.dk/KBA/CAS/106534/?show_KBA=1&portaldesign=1 see KBA here]
*:[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhERkVKS0lNTFRkJWMyJTg3JTdjdiVjMiU4MyU3ZSVjMiU4OHYlYzIlODklN2UlYzIlODQlYzIlODMlYzIlODglNWVZUkk=#K see SDS here]
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Performance
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Performance
Line 58: Line 78:
*Isotropic
*Isotropic
|-
|-
|style="background:LightGrey; color:black"|Etch rates
|style="background:LightGrey; color:black"|Etch rates  
[[/BHF etch rates|See more]]
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Wet thermal oxide:~80nm/min  
*Wet thermal oxide:75-80nm/min  
*PECVD1 (standard):~147nm/min
*TEOS:~265nm/min
*Stoichiometric Si3N4:~0.75nm/min (Morten Bo Mikkelsen, March 2013)
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Wet thermal oxide:~25nm/min  
*Wet thermal oxide:~6nm/min(1%) / 25nm/min(5%) / 52nm/min(10%)
*PECVD1 (standard):~87nm/min
*TEOS:~153nm/min
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Boronfloat and quartz: ~3-4 μm/min
*Boronfloat and quartz: ~3-4 μm/min
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*A little higher etch rates than BHF
*Thermal oxide 80 nm/min
|-
|-
|style="background:LightGrey; color:black"|Lifetime of photoresist
|style="background:LightGrey; color:black"|Lifetime of photoresist
Line 86: Line 102:
|style="background:LightGrey; color:black"|Chemical solution
|style="background:LightGrey; color:black"|Chemical solution
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*BHF 12%HF with Ammoniumflouride
*BHF (12%HF with Ammoniumflouride)
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*5% HF
*1% / 5% HF
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*40% HF
*40% HF
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*SiO etch (BHF with a wetting agent)
*BOE 7:1 Etchant VLSI with Surfactant (BHF with a wetting agent)
|-
|-
|style="background:LightGrey; color:black"|Temperature
|style="background:LightGrey; color:black"|Temperature
Line 109: Line 125:
*Silicon nitride
*Silicon nitride
*Poly silicon
*Poly silicon
*photoresist
*Photoresist
*Blue film
*Blue film
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Silicon nitride
*Silicon nitride
*Poly silicon
*Poly silicon
*photoresist
*Photoresist delaminates
*Blue film
*Blue film
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Photoresist  
*Photoresist delaminates
*Silicon nitride (Only on quartz wafers)  
*Silicon nitride (Only on quartz wafers)  
*Poly silicon (Only on quartz wafers)  
*Poly silicon (Only on quartz wafers)  
Line 125: Line 141:
*Silicon nitride
*Silicon nitride
*Poly silicon
*Poly silicon
*photoresist
*Photoresist
*Blue film
*Blue film
|-
|-
Line 137: Line 153:
<br clear="all" />
<br clear="all" />


<gallery caption="Different places to do wet silicon oxide etch" widths="220px" heights="225px" perrow="5"> image:BHF clean RR3.jpg|BHF clean in Cleanroom3. Wet silicon oxide etch bath positioned to the left in the bench.
<gallery caption="Different places to do wet silicon oxide etch" widths="420px" heights="425px" perrow="5"> image:BHF clean.JPG|BHF in wetbench 04 in D-3 (Oxide etch 2: BHF (clean)). Wet silicon oxide etch bath positioned to the right in the wetbench. This bath can also be used for BHF with wetting agent.  
image:KOH_4tommer.jpg|BHF in Cleanroom 3 (KOH bench 1+2.) The BHF bath is positioned between the two KOH baths. This is primarily used to remove oxide before and after a KOH etch.  
image:KOH_BHF.JPG|BHF in wetbench 01 Si etch in D-3 (Oxide etch 1: BHF). The BHF bath is positioned in the middle of the bench. This is primarily used to remove oxide before and after a Si etch.
image:KOH3 RR4 1.JPG|BHF in Cleanroom 4 (KOH bench 6".) The BHF bath is positioned to the right. This is primarily used to remove oxide before and after a KOH etch.
image:BHF clean.JPG|BHF in wetbench 05 in D-3 (Oxide etch 3: 10% HF). Wet silicon oxide etch bath positioned to the right in the wetbench. This bath can also be used for BHF, BHF with wetting agent or 40% HF on request. This bath is also used for cleaning quarts carriers from the PECVD4 system.
image:BHF-PolySi-Al Etch.jpg|SIO etch bath (BHF with wetting agent) are positioned to the left in the bench in cleanroom 4.  
image:RCA-HF.jpg|HF baths in RCA bench in B-1. These may only be used together with RCA cleaning and furnace processes.
image:Stinkskab RR2.jpg|PP-bath: positioned in the upper right corner of the fumehood in cleanroom 2. </gallery>
</gallery>




Line 152: Line 168:
|-style="background:silver; color:black"
|-style="background:silver; color:black"
!  
!  
! BHF clean in Cleanroom3
! BHF (KOH) in D-3(Oxide etch 1: BHF)
! BHF in Cleanroom3 (KOH bench 1+2)
! BHF clean in D-3 (Oxide etch 2: BHF)
! BHF in Cleanroom4 (KOH bench 6”)
! BHF in RCA Bench
! BHF in RCA Bench
! BHF in PP-bath
! BHF in PP-bath
Line 164: Line 179:
|1-25 wafers at a time
|1-25 wafers at a time
|1-25 wafer at a time
|1-25 wafer at a time
|1-25 wafers at a time
|1-25 wafers at a time
|1-25 wafers at a time
|1-25 wafers at a time
|1-25 wafers at a time
Line 172: Line 186:
|-style="background:LightGrey; color:black"
|-style="background:LightGrey; color:black"
!Size of substrate
!Size of substrate
|2"-4" wafers
|2"-6" wafers
|2"-4" wafers
|2"-6" wafers
|2"-6" wafers
|2"-6" wafers
|2"-6" wafers
Line 182: Line 195:
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
!Allowed materials
!Allowed materials
|
*Silicon
*Poly Silicon
*Silicon Oxide
*Silicon Nitride
*Silicon Oxynitride
*Photoresist
*Blue film
|
|
*Silicon
*Silicon
Line 219: Line 224:
|-style="background:LightGrey; color:black"
|-style="background:LightGrey; color:black"
!Restrictions
!Restrictions
|Wafers have to be cleaned in 7UP or RCA before further processing.
|No wafers with metal are allowed in this bath
|No wafers with metal are allowed in this bath
|Wafers have to be cleaned in 7UP or RCA before further processing.
|Wafers have to be cleaned in 7UP or RCA before further processing.
|Only for wafers with phosphor glass or boron glass that comes directly from one of the furnaces in stack A. All other substrates and material are strictly forbidden to go into the tank.
|Only for wafers with phosphor glass or boron glass that comes directly from one of the furnaces in stack A. All other substrates and material are strictly forbidden to go into the tank.
|None
|None
Line 230: Line 234:
<br clear="all" />
<br clear="all" />


==Comparing different 5% HF baths==
==Comparing different HF baths==
{|border="1" cellspacing="1" cellpadding="3" style="text-align:left;"  
{|border="1" cellspacing="1" cellpadding="3" style="text-align:left;"  
|-
|-
Line 236: Line 240:
|-style="background:silver; color:black"
|-style="background:silver; color:black"
!  
!  
! 5% HF in RCA Bench
! 1% HF in RCA Bench
! 5% HF PP-bath
! 10% HF in D3 wet bench 5 (Oxide etch 3)
! 5% HF Plastic beaker
! 1% HF Plastic beaker


|-  
|-  
Line 251: Line 255:
!Size of substrate
!Size of substrate
|2"-6" wafers
|2"-6" wafers
|2"- 4" wafers or any that fits in a dedicated holder
|2"- 6" wafers or any that fits in a dedicated holder
|2"- 4" wafers or any that fits in a dedicated holder
|2"- 4" wafers or any that fits in a dedicated holder
|-
|-
Line 264: Line 268:
<br clear="all" />
<br clear="all" />


==Comparing different 40% HF baths==
==40% HF==
{|border="1" cellspacing="1" cellpadding="3" style="text-align:left;"  
{|border="1" cellspacing="1" cellpadding="2" style="text-align:left;"  
|-
|-


|-style="background:silver; color:black"
|-style="background:silver; color:black"
!  
!  
! 40% HF PP-bath
! 40% HF in Plastic beaker, only done by Nanolab staff
! 40% HF Plastic beaker


|-  
|-  
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
!Batch size!
!Batch size!
|1-25 wafers at a time
|1 wafer at a time
|1 wafer at a time
|-
|-
Line 282: Line 284:
|-style="background:LightGrey; color:black"
|-style="background:LightGrey; color:black"
!Size of substrate
!Size of substrate
|Any that fits to a dedicated holder
|Any that fits to a dedicated holder
|Any that fits to a dedicated holder
|-
|-
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
!Allowed materials
!Allowed materials
|All materials
|All materials  
|All materials  
|-
|-
Line 294: Line 294:
<br clear="all" />
<br clear="all" />


==SiO etch bath==
==BOE 7:1 Etchant VLSI with Surfactant bath==
{|border="1" cellspacing="1" cellpadding="3" style="text-align:left;"  
{|border="1" cellspacing="1" cellpadding="3" style="text-align:left;"  
|-
|-
Line 300: Line 300:
|-style="background:silver; color:black"
|-style="background:silver; color:black"
!  
!  
! SiO etch bath
! BOE 7:1 Etchant VLSI with Surfactant bath
|-  
|-  
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
Line 320: Line 320:
*Silicon oxides  
*Silicon oxides  
*Photoresist
*Photoresist
 
|-
|-style="background:WhiteSmoke; color:black"
!Remark
|
Amorphous silicon can be used as a mask fro SiO2 etching.<br/>
For very long and deep etches of SiO2/Quartz (several hours/micrometers) <br/>
we have indications that show that it is not good to use the BOE 7:1 Etchant VLSI with Surfactant etch. <br/>
The amorphous silicon has small holes (etch pits) which the BOE 7:1 Etchant VLSI with Surfactant etch penetrates and the SiO2 below is etched.
|-
|-
|}
|}

Latest revision as of 14:31, 15 September 2026

Feedback to this page: click here

Unless anything else is stated, everything on this page, text and pictures are made by DTU Nanolab.

All links to Kemibrug (SDS) and Labmanager Including APV, requires login.

Etch Wet Silicon Oxide Silicon Oxide

Wet Silicon Oxide Etch (BHF, HF and BOE 7:1 Etchant VLSI)

Silicon oxide can be etched using HF. At DTU Nanolab it is mainly used in a buffered version BHF (premixed). You can find safety datasheets on Kemibrug here The BHF has a stable etch rate and is gentle to photoresist due to an almost pH neutral solution which makes photoresist a good masking material for the oxide etch.

BOE 7:1 Etchant VLSI with Surfactant (BHF with wetting agent) can also be used for etching silicon oxide. This is mainly for etching small holes. At DTU Nanolab we do not have BHF with wetting agent in a prepared bath, it's only to be used in fumehoods. It's not very often used and we do not have it as a standard chemical. Please contact DTU Nanolab if you need it.

Wafers with metals or other materials, not allowed in the dedicated oxide etch baths, can be etched using a plastic beaker in Fume hood 01 or 02 (Acids/bases) in D-3. Samples with III-V materials (e.g. InP and GaAs) must be etched in Fume hood 07: III-V Avids/bases in D-3.

The user manual for Oxide etch 1: BHF, APV's and contact information can be found in LabManager by clicking here

The user manual for Oxide etch 2: BHF (clean), APV's and contact information can be found in LabManager by clicking here

The user manual for Oxide etch 3: 10% HF, APV's and contact information can be found in LabManager by clicking here

The user manual for various HF baths in RCA and Fume hoods, APV's and contact information can be found in LabManager by clicking here

Working with HF above 13% is only allowed by Nanolab staff


Process information:
See more etch rates in HF solutions.


Etchant BHF 1% HF / 5% HF / 10% HF 40% HF BOE 7:1 Etchant VLSI with Surfactant
Purpose Etching of silicon oxide
  • Etching of silicon oxide with a stable etch rate
  • Mainly for removing native oxide
  • Mainly for etching deep into borofloat or quartz wafers. Only Nanolab staff are allowed to work with this HF.
  • Etching of silicon oxide - especially for etching small holes
Link to safety APV and SDS (You must be logged in to Kemibrug to view SDSs)
Performance Isotropic
  • Isotropic
  • Isotropic
  • Isotropic
  • Isotropic
Etch rates

See more

  • Wet thermal oxide:75-80nm/min
  • Wet thermal oxide:~6nm/min(1%) / 25nm/min(5%) / 52nm/min(10%)
  • Boronfloat and quartz: ~3-4 μm/min
  • Thermal oxide 80 nm/min
Lifetime of photoresist
  • ~½ hour
  • ~½ hour
  • ~½ hour
  • ~½ hour
Process parameter range Chemical solution
  • BHF (12%HF with Ammoniumflouride)
  • 1% / 5% HF
  • 40% HF
  • BOE 7:1 Etchant VLSI with Surfactant (BHF with a wetting agent)
Temperature
  • Room temperature
  • Room temperature
  • Room temperature
  • Room temperature
Substrates Masking material
  • Silicon nitride
  • Poly silicon
  • Photoresist
  • Blue film
  • Silicon nitride
  • Poly silicon
  • Photoresist delaminates
  • Blue film
  • Photoresist delaminates
  • Silicon nitride (Only on quartz wafers)
  • Poly silicon (Only on quartz wafers)
  • Blue film
  • Chromium and gold
  • Silicon nitride
  • Poly silicon
  • Photoresist
  • Blue film

Life time of the photoresist and blue film in BHF

Photoresist delaminates from the substrate in BHF. For standard photoresist this process starts after about or less than ½ hour but the time can vary with resist pattern. It starts by under etching the photoresist at the edges. The life time can be prolonged a little to ½ hour - 40 minutes if the photoresist is baked at 120oC.

Blue film also has a limited life time in BHF. Blue film is mainly used for back side protecting the wafer while etching on the front side. The life time of Blue film is also about ½ hour.




Comparing different BHF baths

BHF (KOH) in D-3(Oxide etch 1: BHF) BHF clean in D-3 (Oxide etch 2: BHF) BHF in RCA Bench BHF in PP-bath BHF Plastic beaker
Batch size! 1-25 wafers at a time 1-25 wafer at a time 1-25 wafers at a time 1-25 wafers at a time 1-7 wafers at a time
Size of substrate 2"-6" wafers 2"-6" wafers 2"-6" wafers 2"- 4" wafers or any that fits in a dedicated holder 2"- 4" wafers or any that fits in a dedicated holder
Allowed materials
  • Silicon
  • Poly Silicon
  • Silicon Oxide
  • Silicon Nitride
  • Silicon Oxynitride
  • Photoresist
  • Blue film
  • Silicon
  • Poly Silicon
  • Silicon Oxide
  • Silicon Nitride
  • Silicon Oxynitride
  • Photoresist
  • Blue film
  • Silicon
  • Poly Silicon
  • Silicon Oxide
  • Silicon Nitride
  • Silicon Oxynitride
  • All materials
  • All materials
Restrictions Wafers have to be cleaned in 7UP or RCA before further processing. No wafers with metal are allowed in this bath Only for wafers with phosphor glass or boron glass that comes directly from one of the furnaces in stack A. All other substrates and material are strictly forbidden to go into the tank. None None


Comparing different HF baths

1% HF in RCA Bench 10% HF in D3 wet bench 5 (Oxide etch 3) 1% HF Plastic beaker
Batch size! 1-25 wafers at a time 1-25 wafer at a time 1-7 wafers at a time
Size of substrate 2"-6" wafers 2"- 6" wafers or any that fits in a dedicated holder 2"- 4" wafers or any that fits in a dedicated holder
Allowed materials Only for wafers that are being RCA cleaned All materials All materials


40% HF

40% HF in Plastic beaker, only done by Nanolab staff
Batch size! 1 wafer at a time
Size of substrate Any that fits to a dedicated holder
Allowed materials All materials


BOE 7:1 Etchant VLSI with Surfactant bath

BOE 7:1 Etchant VLSI with Surfactant bath
Batch size! 1-25 wafers at a time
Size of substrate 4" wafers
Allowed materials
  • Silicon
  • Poly silicon
  • Silicon nitrides
  • Silicon oxynitrides
  • Silicon oxides
  • Photoresist
Remark

Amorphous silicon can be used as a mask fro SiO2 etching.
For very long and deep etches of SiO2/Quartz (several hours/micrometers)
we have indications that show that it is not good to use the BOE 7:1 Etchant VLSI with Surfactant etch.
The amorphous silicon has small holes (etch pits) which the BOE 7:1 Etchant VLSI with Surfactant etch penetrates and the SiO2 below is etched.