Specific Process Knowledge/Etch/ICP Metal Etcher/silicon nitride: Difference between revisions
Appearance
mNo edit summary |
|||
| (12 intermediate revisions by 2 users not shown) | |||
| Line 1: | Line 1: | ||
===Slow etch of silicon nitride with resist as masking material - with | {{cc-nanolab}} | ||
This recipe can be used for slow etching of silicon nitride with resist as masking material | |||
Here are some test results presented. | '''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/ICP_Metal_Etcher/silicon_nitride click here]''' | ||
<br> | |||
==Slow etch of silicon nitride with resist as masking material - on 6" carrier wafer with recess == | |||
{{CC-bghe2}} <br> | |||
This recipe can be used for slow etching of silicon nitride with resist as masking material. Here are some test results presented. The same recipe is being used for SiO2, see the result for that [[Specific Process Knowledge/Etch/ICP Metal Etcher/silicon oxide#Slow etch of SiO2 with resist as masking material-using a 6.22 carrier wafer with recess|here]] | |||
{| border="2" cellspacing="2" cellpadding="3" | {| border="2" cellspacing="2" cellpadding="3" | ||
!Parameter | !Parameter | ||
! | !A slow etch with carrier | ||
|- | |- | ||
|Coil Power [W] | |Coil Power [W] | ||
| Line 30: | Line 37: | ||
{| border="2" cellspacing="2" cellpadding="3" | {| border="2" cellspacing="2" cellpadding="3" | ||
!Results | !Results | ||
!Test on wafer with 20% load, by Izzet Yildiz @Nanotech | !Test on wafer with 20% load, ''by Izzet Yildiz @Nanotech'' | ||
!Test by BGHE @nanolab | |||
|- | |- | ||
|Etch rate of LPCVD nitride | |Etch rate of LPCVD nitride | ||
|'''60-65 nm/min (20% etch load) (Feb. | |'''60-65 nm/min (20% etch load) (Feb. 2014)''' | ||
| | |||
|- | |- | ||
|Selectivity to resist [SiN : AZ resist] | |Selectivity to resist [SiN : AZ resist] | ||
|'''1:0.75''' | |'''1:0.75''' | ||
| | |||
|- | |- | ||
|Wafer uniformity (100mm) | |Wafer uniformity (100mm) | ||
|'''?''' | |'''?''' | ||
| | |||
|- | |- | ||
|Profile [<sup>o</sup>] | |Profile [<sup>o</sup>] | ||
|? | |? | ||
| | |||
|- | |- | ||
|Wafer uniformity map (click on the image to view a larger image) | |Wafer uniformity map (click on the image to view a larger image) | ||
|not measured | |not measured | ||
| | |||
|- | |- | ||
|SEM profile images | |SEM profile images | ||
|Not measured | |Not measured | ||
| | |||
|- | |||
|Etch rate in Barc | |||
| | |||
|~50 nm/min (Date: 2014-09-09) | |||
|- | |||
|Etch rate in KRF resist | |||
| | |||
|~40 nm/min (Date: 2014-09-09) | |||
|- | |- | ||
|} | |} | ||
<br/> | <br/> | ||