Jump to content

Specific Process Knowledge/Thin film deposition/Deposition of Silicon Nitride/Deposition of Silicon Nitride using PECVD: Difference between revisions

From LabAdviser
Bghe (talk | contribs)
Bghe (talk | contribs)
 
(95 intermediate revisions by 5 users not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Silicon_Nitride/Deposition_of_Silicon_Nitride_using_PECVD click here]'''
{{cc-nanolab}}


'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Silicon_Nitride/Deposition_of_Silicon_Nitride_using_PECVD click here]''' <br>


At the moment DANCHIP has 3 PECVDs that can deposite silicon nitride and silicon oxynitride. PECVD1 and PECVD3 are for silicon based processing. PECVD2 is for III-V processing and will be describes under III-V processing. Look at the [[Specific Process Knowledge/Thin film deposition/PECVD|PECVD]] page to learn more about the PECVDs at DANCHIP. All though PECVD1 and PECVD3 are very much alike you cannot count on the a recipe on one system will give exactly the same results on the other system.


==Recipes on PECVD1 for deposition of silicon nitride and silicon oxynitride==
=Deposition of Silicon Nitride using PECVD=
===Recipes===
 
{| border="1" cellspacing="0" cellpadding="7"
At the moment DTU Nanolab has 2 PECVDs that can deposit silicon nitride and silicon oxynitride. PECVD4 is for clean silicon based and III-V based samples. PECVD3 is for silicon based samples but here up 5% (4 cm2) wafer coverage of other materials as metals are allowed (under some conditions even more). Look at the [[Specific Process Knowledge/Thin film deposition/PECVD|PECVD]] page to learn more about the PECVDs at DTU Nanolab. All though PECVD3 and PECVD4 are very much alike you cannot count on the a recipe on one system will give exactly the same results on the other system.
 
== Deposition of SiN with PECVD4 ==
{| border="1" cellspacing="2" cellpadding="2" colspan="3"
|bgcolor="#98FB98" |'''Quality Control (QC) for PECVD4 '''
|-
|
*[http://labmanager.dtu.dk/d4Show.php?id=5093&mach=395 The QC procedure for PECVD4 - requires login]<br>
*[https://labmanager.dtu.dk/view_binary.php?type=data&mach=395 The newest QC data for PECVD4 - requires login]<br>
{| {{table}}
| align="center" |
{| border="1" cellspacing="1" cellpadding="2"  align="center" style="width:200px"
 
! QC Recipe:
! QCNITRIDE=HFSIN
|-
| SiH<sub>4</sub> flow
|40 sccm
|-
|NH<sub>3</sub> flow
|55 sccm
|-
|-
|Recipe name
|N<sub>2</sub> flow
|SiH4 flow [sccm]
|1960 sccm
|NH3 flow [sccm]
|N2 flow [sccm]
|Pressure [mTorr]
|Power [W]
|Description
|-  
|-  
|1nitride
|Pressure
|30
|900 mTorr
|20
|-
|1000
|RF-power
|500
|80
|
|
HF: 20 W 
|-
|}
| align="center" valign="top"|
{| border="2" cellspacing="1" cellpadding="2" align="center" style="width:500px"
!QC limits
!PECVD4
|-
|-
|1nit_std
|Deposition rate
|40
|11.0-13.2 nm/min
|20
|-
|1960
|Non-uniformity
|550
|<3.0 %
|60
|-
|Process control recipe
|Refractive Index
|1.988 - 2.018
|}
|-
|-
|}
|}
|}
<nowiki>*</nowiki> Due to recent oscillations on the QC nitride recipe (HF), new tests were performed. Learn more about it under [[Deposition of SiN with PECVD4/NEW TESTS QC|NEW TESTS QC]] . (Still under development.)


===Expected results===
{| border="1" cellspacing="2" cellpadding="2"
{| border="1" cellspacing="0" cellpadding="5"
|-style="background:Black; color:White"
!|Recipe
!|Dep. rate [nm/min]
!|RI
!|Unif. [%]
!|Stress [MPa]
!|Comments
!|SiH4 [sccm]
!|NH3 [sccm]
!|N2O [sccm]
!|N2 [sccm]
!|Pressure [mTorr]
!|Power [W]
!|Load
!|Tune
!|Time [mm:ss]
!|Tested
|-
|MF SIN<!-- Recipe -->
|12.9-13.0 nm/min <br> 11.7 nm/min (''kabi 2019-03-01'')<!-- Dep. rate [nm/min] -->
|2.038-2.044<!-- RI -->
|&plusmn; 1.7%<!-- Unif. [%] -->
|157 MPa <!-- Stress [MPa] -->
|[[/MF_SiN results|more results]]<!-- Comments -->
|40<!-- SiH4 [sccm] -->
|40<!-- NH3 [sccm] -->
|<!-- N2O [sccm] -->
|1920<!-- N2 [sccm] -->
|900 mTorr<!-- Pressure [mTorr] -->
|20HF6"/20LF2"<!-- Power [W] -->
|<!-- Load -->
|<!-- Tune -->
|10:00/60:00(stress)<!-- Time [mm:ss] -->
|February 2017 Berit Herstrøm @DTU Nanolab (bghe)<!--Tested -->
|-
|-
|MF SIN2<!-- Recipe -->
|44.3 nm/min <!-- Dep. rate [nm/min] -->
|2.01-2.02 <!-- RI -->
|&plusmn; 2.7%<!-- Unif. [%] -->
|? MPa <!-- Stress [MPa] -->
|<!-- Comments -->
|30<!-- SiH4 [sccm] -->
|30<!-- NH3 [sccm] -->
|<!-- N2O [sccm] -->
|1470<!-- N2 [sccm] -->
|850 mTorr<!-- Pressure [mTorr] -->
|100HF8.2"/100LF2.2"<!-- Power [W] -->
|<!-- Load -->
|<!-- Tune -->
|10:00<!-- Time [mm:ss] -->
|February 2020 bghe<!--Tested -->
|-
|-
|Recipe name
|LF SIN<!-- Recipe -->
|Deposition rate [nm/min]
|40-43 nm/min<!-- Dep. rate [nm/min] -->
|RI
|1.983-1.984<!-- RI -->
|Uniformity [%]
|&plusmn; 3.9-4.4%<!-- Unif. [%] -->
|Stress [MPa]
|Compressive: 565.4 MPa<!-- Stress [MPa] -->
|BHF etch rate [Å/min]
|<!-- Comments -->
|Comments
|40<!-- SiH4 [sccm] -->
|-  
|20<!-- NH3 [sccm] -->
|1nitride
|<!-- N2O [sccm] -->
|
|1960<!-- N2 [sccm] -->
|
|550 mTorr<!-- Pressure [mTorr] -->
|
|60LF<!-- Power [W] -->
|
|<!-- Load -->
|
|<!-- Tune -->
|
|2:00/23:00(stress)<!-- Time [mm:ss] -->
|February 2017 bghe<!--Tested -->
|-
|-
|1nit_std
|HF SiN <!-- Recipe -->
|~32
|12.2-12.4 nm/min<!-- Dep. rate [nm/min] -->
|1.89
|2.017-2.021<!-- RI -->
|~1
|&plusmn; 1.2-1.6%<!-- Unif. [%] -->
|
|Tensile: 431.6 MPa<!-- Stress [MPa] -->
|~700
|<!-- Comments -->
|The latest measured values can be seen in the process control sheet in LabManager
|40<!-- SiH4 [sccm] -->
|55<!-- NH3 [sccm] -->
|<!-- N2O [sccm] -->
|1960<!-- N2 [sccm] -->
|900 mTorr<!-- Pressure [mTorr] -->
|20 W<!-- Power [W] -->
|<!-- Load -->
|<!-- Tune -->
|10:00/56:00(stress)<!-- Time [mm:ss] -->
|February 2017 bghe<!--Tested -->
|-
|-
|}
|}




<br clear="all" />


<br clear="all" />


==Recipes on PECVD3 for deposition of silicon nitride and silicon oxynitride==
==Recipes on PECVD3 for deposition of silicon nitride==


{| border="1" cellspacing="2" cellpadding="2" colspan="3"
{| border="1" cellspacing="2" cellpadding="2" colspan="3"
Line 72: Line 163:
|-
|-
|
|
*[http://labmanager.danchip.dtu.dk/d4Show.php?id=1402&mach=106 The QC procedure for PECVD3]<br>
*[http://labmanager.dtu.dk/d4Show.php?id=1402&mach=106 The QC procedure for PECVD3 - requires login]<br>
*[http://www.labmanager.danchip.dtu.dk/view_binary.php?type=data&mach=106 The newest QC data for PECVD3]<br>
*[https://labmanager.dtu.dk/view_binary.php?type=data&mach=106 The newest QC data for PECVD3 - requires login]<br>
{| {{table}}
{| {{table}}
| align="center" |  
| align="center" |  
Line 91: Line 182:
|-  
|-  
|Pressure
|Pressure
|650 mTorr
|845 mTorr
|-
|-
|RF-power
|RF-power
|
|
*LF: 20 W 2s
*HF: 100 W 7.8s
*HF: 20 W 6s
*LF: 100 W 2.2s
|-
|-
|}
|}
Line 104: Line 195:
!PECVD3
!PECVD3
|-
|-
|Depoition rate
|Deposition rate
|10.4 - 13.0 nm/min
|~40 nm/min
|-
|-
|Non-uniformity
|Non-uniformity
|<2.0 %
|<3.0 %
|-
|-
|Refractive Index
|Refractive Index
|1.909 - 2.028
|2.02 - 2.04
|}
|}
|-
|-
|}
|}
|}
|}


===Recipes===
===Recipes===
Line 128: Line 218:
|Power [W]
|Power [W]
|Description
|Description
|-
|MFSiNLS2
|30
|30
|1470
|845
|100HF 7.8s
100LF 2.2s
|Low stress nitride - standard recipe. The latest measured values can be seen in the process control sheet in LabManager.
|-  
|-  
|MFSiNLS
|MFSiNLS
Line 135: Line 235:
|650
|650
|20HF 6s  
|20HF 6s  
20LF 2s
30LF 2s
|Low stress nitride - standard recipe. The latest measured values can be seen in the process control sheet in LabManager.
|Low stress nitride - old standard recipe. This one is not running well any more.
|-
|-
|LFSiN
|LFSiN
Line 167: Line 267:
|KOH etch rate [Å/min]
|KOH etch rate [Å/min]
|BHF etch rate [Å/min]
|BHF etch rate [Å/min]
|See more
|-  
|-  
|MFSiNLS2
|~422 (''bghe Feb 2016'')
|~2.03
|~2
|~6 (''bghe Feb 2016'')
|~2.1 (''bghe Feb 2016'')
|~?
|[[/PECVD3: Low stress nitride testing|see more results]]
|-
|MFSiNLS
|MFSiNLS
|~107
|~107
Line 175: Line 285:
|~2.5
|~2.5
|~250
|~250
|.
|-
|-
|LFSiN
|LFSiN
Line 181: Line 292:
|~3
|~3
|~-630
|~-630
|.
|.
|.
|.
|.
Line 189: Line 301:
|~2
|~2
|~460
|~460
|.
|.
|.
|.
|.
|-
|-
|}
|}
==Recipes on PECVD2 for Deposition of Silicon Nitride==
'''<span style="color:Red">Expired Recipes! The PECVD2 has been decomissioned and is no longer available.</span>'''
===Recipes===
{| border="1" cellspacing="0" cellpadding="7"
|-
|Recipe name
|SiH4 flow [sccm]
|NH3 flow [sccm]
|N2 flow [sccm]
|Pressure [mTorr]
|Power [W]
|Description
|-
|SINSTD80
|30
|20
|1000
|500
|80
|
|-
|SINSTD96
|30
|20
|1000
|500
|96
|
|-
|1SiN
|40
|20
|1000
|700
|150
|
|-
|}
===Expected results===
{| border="1" cellspacing="0" cellpadding="5"
|-
|Recipe name
|Deposition rate [nm/min]
|RI
|Uniformity [%]
|Stress [MPa]
|BHF etch rate [Å/min]
|Comments
|-
|1SiN
|
Deposition rate in the middle of two wafers: '''49nm/min+-1nm/min''' (2015-04-24 BGHE) <br>
In the middel: '''72.6-76.4 nm/min''' (2014-08-13 BGHE) ''Old shower head''<br>
Variation over 3 wafers: '''71.4-78.6 nm/min''' (2014-08-13 BGHE) ''Old shower head''
|
|
'''~2-4%''' (2015-04-24 BGHE)<br>
'''~5%''' in the middel (4") (2014-08-13 BGHE) ''Old shower head''<br>
'''~10%''' over 3 wafers (2014-08-13 BGHE) ''Old shower head''
|
|
|
|-
|SINSTD80
|68nm/min (2014-07-07 JML)- unstable deposition rate
|
|
|
|
|
|-
|SINSTD96 - unstable deposition rate
|
|
|
|
|
|
|-
|}
==Recipes on PECVD1 for Deposition of Silicon Nitride==
'''<span style="color:Red">Expired Recipes! The PECVD1 has been decomissioned and is no longer available.</span>'''
===Recipes===
{| border="1" cellspacing="0" cellpadding="7"
|-
|Recipe name
|SiH4 flow [sccm]
|NH3 flow [sccm]
|N2 flow [sccm]
|Pressure [mTorr]
|Power [W]
|Description
|-
|1nitride
|30
|20
|1000
|500
|80
|
|-
|1nit_std
|40
|20
|1960
|550
|60
|Process control recipe
|-
|}
===Expected results===
{| border="1" cellspacing="0" cellpadding="5"
|-
|Recipe name
|Deposition rate [nm/min]
|RI
|Uniformity [%]
|Stress [MPa]
|BHF etch rate [Å/min]
|Comments
|-
|1nitride
|
|
|
|
|
|
|-
|1nit_std
|~32
|1.89
|~1
|
|~700
|The latest measured values can be seen in the process control sheet in LabManager
|-
|}
=Oxynitrides=
The recipe for making oxynitrides will depend on what kind of oxynitride you need. If you need a little higher refractive index than SiO2 then start with an SiO2 recipe and then add NH3 until the right refractive index is obtained. If you need very high refractive index a little lower than for silicon nitride then it is probably better to start with a silicon nitride recipe and add a some N2O until you get the right refractive index.
We had a Ph.d student long time ago Klaus Bo Mogensen that did the first. You can find his ph.d. thesis here: [https://findit.dtu.dk/en/catalog?author=Mogensen&q=title%3A%28Integration+of+Planar+Waveguides+for+Optical+Detection+in+Microfabricated+Analytical+Devices%29 Integration of Planar Waveguides for Optical Detection in Microfabricated Analytical Devices]
Berit H. has the thesis in her office.

Latest revision as of 10:23, 30 October 2025

The content on this page, including all images and pictures, was created by DTU Nanolab staff, unless otherwise stated.

Feedback to this page: click here


Deposition of Silicon Nitride using PECVD

At the moment DTU Nanolab has 2 PECVDs that can deposit silicon nitride and silicon oxynitride. PECVD4 is for clean silicon based and III-V based samples. PECVD3 is for silicon based samples but here up 5% (4 cm2) wafer coverage of other materials as metals are allowed (under some conditions even more). Look at the PECVD page to learn more about the PECVDs at DTU Nanolab. All though PECVD3 and PECVD4 are very much alike you cannot count on the a recipe on one system will give exactly the same results on the other system.

Deposition of SiN with PECVD4

Quality Control (QC) for PECVD4
QC Recipe: QCNITRIDE=HFSIN
SiH4 flow 40 sccm
NH3 flow 55 sccm
N2 flow 1960 sccm
Pressure 900 mTorr
RF-power

HF: 20 W

QC limits PECVD4
Deposition rate 11.0-13.2 nm/min
Non-uniformity <3.0 %
Refractive Index 1.988 - 2.018

* Due to recent oscillations on the QC nitride recipe (HF), new tests were performed. Learn more about it under NEW TESTS QC . (Still under development.)


Recipe Dep. rate [nm/min] RI Unif. [%] Stress [MPa] Comments SiH4 [sccm] NH3 [sccm] N2O [sccm] N2 [sccm] Pressure [mTorr] Power [W] Load Tune Time [mm:ss] Tested


MF SIN 12.9-13.0 nm/min
11.7 nm/min (kabi 2019-03-01)
2.038-2.044 ± 1.7% 157 MPa more results 40 40 1920 900 mTorr 20HF6"/20LF2" 10:00/60:00(stress) February 2017 Berit Herstrøm @DTU Nanolab (bghe)
MF SIN2 44.3 nm/min 2.01-2.02 ± 2.7% ? MPa 30 30 1470 850 mTorr 100HF8.2"/100LF2.2" 10:00 February 2020 bghe
LF SIN 40-43 nm/min 1.983-1.984 ± 3.9-4.4% Compressive: 565.4 MPa 40 20 1960 550 mTorr 60LF 2:00/23:00(stress) February 2017 bghe
HF SiN 12.2-12.4 nm/min 2.017-2.021 ± 1.2-1.6% Tensile: 431.6 MPa 40 55 1960 900 mTorr 20 W 10:00/56:00(stress) February 2017 bghe




Recipes on PECVD3 for deposition of silicon nitride

Quality Controle (QC) for PECVD3
QC Recipe: QCNITRIDE
SiH4 flow 30 sccm
NH3 flow 30 sccm
N2 flow 1470 sccm
Pressure 845 mTorr
RF-power
  • HF: 100 W 7.8s
  • LF: 100 W 2.2s
QC limits PECVD3
Deposition rate ~40 nm/min
Non-uniformity <3.0 %
Refractive Index 2.02 - 2.04

Recipes

Recipe name SiH4 flow [sccm] NH3 flow [sccm] N2 flow [sccm] Pressure [mTorr] Power [W] Description
MFSiNLS2 30 30 1470 845 100HF 7.8s

100LF 2.2s

Low stress nitride - standard recipe. The latest measured values can be seen in the process control sheet in LabManager.
MFSiNLS 30 30 1470 650 20HF 6s

30LF 2s

Low stress nitride - old standard recipe. This one is not running well any more.
LFSiN 30 15 1470 550 60LF Compressive stress
HFSiN 30 42 1470 900 20HF Tensile stress

LF=Low Frequency HF=High Frequency MF=Mixed Frequency SiN=Silicon Nitride LS=Low Stress

Expected results

Recipe name Deposition rate [Å/min] RI Uniformity [%]
[Std./mean]
Stress [MPa] KOH etch rate [Å/min] BHF etch rate [Å/min] See more
MFSiNLS2 ~422 (bghe Feb 2016) ~2.03 ~2 ~6 (bghe Feb 2016) ~2.1 (bghe Feb 2016) ~? see more results
MFSiNLS ~107 ~1.99 ~4 ~-30 ~2.5 ~250 .
LFSiN ~550 ~1.96 ~3 ~-630 . . .
HFSiN ~130 ~1.97 ~2 ~460 . . .

Recipes on PECVD2 for Deposition of Silicon Nitride

Expired Recipes! The PECVD2 has been decomissioned and is no longer available.

Recipes

Recipe name SiH4 flow [sccm] NH3 flow [sccm] N2 flow [sccm] Pressure [mTorr] Power [W] Description
SINSTD80 30 20 1000 500 80
SINSTD96 30 20 1000 500 96
1SiN 40 20 1000 700 150

Expected results

Recipe name Deposition rate [nm/min] RI Uniformity [%] Stress [MPa] BHF etch rate [Å/min] Comments
1SiN

Deposition rate in the middle of two wafers: 49nm/min+-1nm/min (2015-04-24 BGHE)
In the middel: 72.6-76.4 nm/min (2014-08-13 BGHE) Old shower head
Variation over 3 wafers: 71.4-78.6 nm/min (2014-08-13 BGHE) Old shower head

~2-4% (2015-04-24 BGHE)
~5% in the middel (4") (2014-08-13 BGHE) Old shower head
~10% over 3 wafers (2014-08-13 BGHE) Old shower head

SINSTD80 68nm/min (2014-07-07 JML)- unstable deposition rate
SINSTD96 - unstable deposition rate

Recipes on PECVD1 for Deposition of Silicon Nitride

Expired Recipes! The PECVD1 has been decomissioned and is no longer available.

Recipes

Recipe name SiH4 flow [sccm] NH3 flow [sccm] N2 flow [sccm] Pressure [mTorr] Power [W] Description
1nitride 30 20 1000 500 80
1nit_std 40 20 1960 550 60 Process control recipe

Expected results

Recipe name Deposition rate [nm/min] RI Uniformity [%] Stress [MPa] BHF etch rate [Å/min] Comments
1nitride
1nit_std ~32 1.89 ~1 ~700 The latest measured values can be seen in the process control sheet in LabManager

Oxynitrides

The recipe for making oxynitrides will depend on what kind of oxynitride you need. If you need a little higher refractive index than SiO2 then start with an SiO2 recipe and then add NH3 until the right refractive index is obtained. If you need very high refractive index a little lower than for silicon nitride then it is probably better to start with a silicon nitride recipe and add a some N2O until you get the right refractive index.

We had a Ph.d student long time ago Klaus Bo Mogensen that did the first. You can find his ph.d. thesis here: Integration of Planar Waveguides for Optical Detection in Microfabricated Analytical Devices

Berit H. has the thesis in her office.