SU-8 can be etched by a oxygen plasma with a small amount of SF<sub>6</sub> to remove the antimony present from the photo initiator. Etching of SU-8 has been developed on the ASE and was tested as a mask less reduction of | SU-8 can be etched by a oxygen plasma with a small amount of SF<sub>6</sub> to remove the antimony present from the photo initiator. Etching of SU-8 has been developed on the ASE and was tested as a mask less reduction of patterns defined by photo lithography. Two processes are available, a high and a low anisotropic etch for use as etching or thinning of structures. | ||
* High anisotropic etch: etch rate ~400nm/min, anisotropy ~0.8 | * High anisotropic etch: etch rate ~400nm/min, anisotropy ~0.8 | ||
| Line 10: | Line 14: | ||
{| border="2" cellpadding="2" cellspacing="1" style="text-align:center;" | {| border="2" cellpadding="2" cellspacing="1" style="text-align:center;" | ||
|+ '''SU8aniso and SU8iso etches''' by khara@ | |+ '''SU8aniso and SU8iso etches''' by khara@nanolab | ||
|- | |- | ||
! Parameter | ! Parameter | ||
| Line 55: | Line 59: | ||
===SU8iso=== | ===SU8iso=== | ||
The SU8iso etch was developed for thinning of lithography defined structures to gain higher aspect ratio or thinner structures than possible with photo lithography. | The SU8iso etch was developed for thinning of lithography defined structures to gain higher aspect ratio or thinner structures than possible with photo lithography. | ||
==Roughness and antimony effects in SU-8 etching== | |||
{| border="1" cellspacing="1" cellpadding="2" align="left" | |||
! SU-8 lines by lithography | |||
! Oxygen etch | |||
! SU8aniso | |||
! SU8iso | |||
|- | |||
|[[Image:SU8-noetch Q13.jpg|200x200px]] | |||
|[[Image:SU8-oxygen-etch_Q12.jpg|200x200px]] | |||
|[[Image:SU8-SU8aniso_R15.jpg|200x200px]] | |||
|[[Image:SU8-SU8iso_R13.jpg|200x200px]] | |||
|- | |||
|No etching | |||
|Etch | |||
*O<sub>2</sub> flow [sccm]:99 | |||
*SF<sub>6</sub> flow [sccm]:0 | |||
*Pressure [mTorr]:20 | |||
*Coil power [W]:800 | |||
*Platen power [W]:30 | |||
*Temperature [°C]:10 | |||
|Etch | |||
*O<sub>2</sub> flow [sccm]:99 | |||
*SF<sub>6</sub> flow [sccm]:17 | |||
*Pressure [mTorr]:40 | |||
*Coil power [W]:800 | |||
*Platen power [W]:30 | |||
*Temperature [°C]:30 | |||
|Etch | |||
*O<sub>2</sub> flow [sccm]:99 | |||
*SF<sub>6</sub> flow [sccm]:14 | |||
*Pressure [mTorr]:20 | |||
*Coil power [W]:800 | |||
*Platen power [W]:0 | |||
*Temperature [°C]:10 | |||
|} | |||
Latest revision as of 12:32, 31 March 2025
Etching of SU-8
SU-8 can be etched by a oxygen plasma with a small amount of SF6 to remove the antimony present from the photo initiator. Etching of SU-8 has been developed on the ASE and was tested as a mask less reduction of patterns defined by photo lithography. Two processes are available, a high and a low anisotropic etch for use as etching or thinning of structures.
- High anisotropic etch: etch rate ~400nm/min, anisotropy ~0.8
- Low anisotropic etch: etch rate ~170nm/min, anisotropy ~0.3
Recipes in ASE
SU8aniso
The anisotropic SU8aniso etch was design to etch structures in SU-8 with a low roughness of the etched surface, however it has not been tested with any mask material. For a polymeric mask a low selectivity is expected. The etch rate was measured to around 400 nm/min, but will depend on wafer coverage. The surface layer concentration of antimony (Sb) after etch is expected to be below 2%.
| Parameter | SU8aniso etch | SU8iso etch |
|---|---|---|
| O2 (sccm) | 99 | 99 |
| SF6 (sccm) | 17 | 14 |
| Pressure (mTorr) | 40 | 20 |
| Coil power (W) | 800 | 800 |
| Platen power (W) | 30 | 0 |
| Temperature (oC) | 30 | 10 |
| Etch rate (nm/min) | ~400 | ~170 |
| anisotropy | ~0.8 | ~0.3 |
| Sb in surface layer (%) | <2 | <2.75 |
SU8iso
The SU8iso etch was developed for thinning of lithography defined structures to gain higher aspect ratio or thinner structures than possible with photo lithography.