=Etch slow (this was tested in 2012 by ''bghe@nanolab'')= | |||
This process development was done to find an etch recipe that is so gentle that the resist masking material can be removed with acetone + ultrasound within hopefully 10min. This is important when a metal is to be etched as this cannot withstand plasma ashing (to remove reist mask) after the etch. | |||
This process development | |||
{| border="2" cellspacing="2" cellpadding="3" | {| border="2" cellspacing="2" cellpadding="3" |
Latest revision as of 15:44, 6 February 2023
Feedback to this page: click here
This page is written by Berit Herstrøm @ DTU Nanolab (BGHE) if nothing else is stated
Etch slow (this was tested in 2012 by bghe@nanolab)
This process development was done to find an etch recipe that is so gentle that the resist masking material can be removed with acetone + ultrasound within hopefully 10min. This is important when a metal is to be etched as this cannot withstand plasma ashing (to remove reist mask) after the etch.
Parameter | Si etch test1 | Si etch test2 | Si etch test3 |
---|---|---|---|
Important note | This recipe must only be run for 5 min, otherwise the beam acc. current will incrase above 20 | ||
Neutalizer current [mA] | 450 | 250 | 450 |
RF Power [W] | 1200 | 1000 | 1200 |
Beam current [mA] | 400 | 200 | 400 |
Beam voltage [V] | 400 | 200 | 400 |
Beam accelerator voltage | 400 | 200 | 400 |
Ar flow to neutralizer [sccm] | 6.0 | 6.0 | 6.0 |
Ar flow to beam [sccm] | 6.0 | 6.0 | 6.0 |
Rotation speed [rpm] | 20 | 20 | 20 |
Stage angle [degrees] | 10 | 10 | 10 |
Platen temp. [dg. Celcius] | 15 | 15 | 15 |
He cooling pressure [mTorr] | 37.5 | 37.5 | 37.5 |
Etch material | Si | Si | Si |
Results | vvv | vvv | vvv |
Etch time [min] | 40 | 40 | 7:15 |
Etch rate in Si [nm/min] | 19.7 | 3.58 | 19.3 |
Total time in Acetone + ultrasound [min] | 17 | 10 | 20 |
Was the resist completely removed after acetone + ultrasound? | no | yes | yes (almost) |