Specific Process Knowledge/Etch/Wet Silicon Oxide Etch (BHF): Difference between revisions
| (142 intermediate revisions by 9 users not shown) | |||
| Line 1: | Line 1: | ||
'''Feedback to this page''': '''[mailto: | '''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/Wet_Silicon_Oxide_Etch_(BHF) click here]''' | ||
'''''Unless anything else is stated, everything on this page, text and pictures are made by DTU Nanolab.''''' | |||
'''''All links to Kemibrug (SDS) and Labmanager Including APV, requires login.''''' | |||
[[index.php?title=Category:Equipment|Etch Wet Silicon Oxide]] | |||
[[index.php?title=Category:Etch (Wet) bath|Silicon Oxide]] | |||
Silicon | ==Wet Silicon Oxide Etch (BHF, HF and BOE 7:1 Etchant VLSI)== | ||
Silicon oxide can be etched using HF. At DTU Nanolab it is mainly used in a buffered version BHF (premixed). You can find safety datasheets on Kemibrug [http://kemibrug.dk here] The BHF has a stable etch rate and is gentle to photoresist due to an almost pH neutral solution which makes photoresist a good masking material for the oxide etch. | |||
BOE 7:1 Etchant VLSI with Surfactant (BHF with wetting agent) can also be used for etching silicon oxide. This is mainly for etching small holes. At DTU Nanolab we do not have BHF with wetting agent in a prepared bath, it's only to be used in fumehoods. It's not very often used and we do not have it as a standard chemical. Please contact DTU Nanolab if you need it. | |||
Wafers with metals or other materials, not allowed in the dedicated oxide etch baths, can be etched using a '''plastic beaker''' in Fume hood 01 or 02 (Acids/bases) in D-3. Samples with III-V materials (e.g. InP and GaAs) must be etched in Fume hood 07: III-V Avids/bases in D-3. | |||
<br> | |||
'''The user manual for Oxide etch 1: BHF, APV's and contact information can be found in LabManager''' [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=389 by clicking here] | |||
'''The user manual for Oxide etch 2: BHF (clean), APV's and contact information can be found in LabManager''' [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=378 by clicking here] | |||
'''The user manual for Oxide etch 3: 10% HF, APV's and contact information can be found in LabManager''' [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=380 by clicking here] | |||
'''The user manual for various HF baths in RCA and Fume hoods, APV's and contact information can be found in LabManager''' [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=64 by clicking here] | |||
'''<big>Working with HF above 13% is only allowed by Nanolab staff</big>''' | |||
<!-- remember to remove the type of documents that are not present --> | |||
'''Process information:''' <br> | |||
See more [[/BHF etch rates|etch rates]] in HF solutions. | |||
{| border="2" cellspacing="0" cellpadding="2" | {| border="2" cellspacing="0" cellpadding="2" | ||
!colspan="2" border="none" style="background:silver; color:black;" align="center"| | !colspan="2" border="none" style="background:silver; color:black;" align="center"|Etchant | ||
|style="background:WhiteSmoke; color:black"|<b> | |style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Etch/Wet_Silicon_Oxide_Etch_(BHF)#Comparing_different_BHF_baths|BHF]]</b> | ||
|style="background:WhiteSmoke; color:black"|<b> | |style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Etch/Wet_Silicon_Oxide_Etch_(BHF)#Comparing_different_5.25_HF_baths|1% HF / 5% HF / 10% HF]]</b> | ||
|style="background:WhiteSmoke; color:black"|<b> | |style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Etch/Wet_Silicon_Oxide_Etch_(BHF)#Comparing_different_40.25_HF_baths|40% HF]]</b> | ||
|style="background:WhiteSmoke; color:black"|<b> | |style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Etch/Wet_Silicon_Oxide_Etch_(BHF)#SiO_etch_bath|BOE 7:1 Etchant VLSI with Surfactant]]</b> | ||
|- | |- | ||
!style="background:silver; color:black;" align="center" width="60" rowspan="2"|Purpose | !style="background:silver; color:black;" align="center" width="60" rowspan="2"|Purpose | ||
|style="background:LightGrey; color:black"| | |style="background:LightGrey; color:black"|Etching of silicon oxide | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
* | *Etching of silicon oxide with a stable etch rate | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
* | *Mainly for removing native oxide | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
* | *Mainly for etching deep into borofloat or quartz wafers. '''Only Nanolab staff are allowed to work with this HF'''. | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
* | *Etching of silicon oxide - especially for etching small holes | ||
|- | |- | ||
|style="background:LightGrey; color:black"|Link to safety APV and | |style="background:LightGrey; color:black"|Link to safety APV and SDS (You must be logged in to Kemibrug to view SDSs) | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
*:[http:// | *:[http://labmanager.nanolab.dtu.dk/d4Show.php?id=1897&mach=64 see APV here] | ||
*:[ | *:[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhESkhKSUxMVGQlYzIlODclN2N2JWMyJTgzJTdlJWMyJTg4diVjMiU4OSU3ZSVjMiU4NCVjMiU4MyVjMiU4OCU1ZVlSSQ==#K see SDS here] | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
*:[http:// | *:[http://labmanager.danchip.dtu.dk/d4Show.php?id=1897&mach=64 see APV here] | ||
*:[ | *:[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhERkZMSkhFR1RkJWMyJTg3JTdjdiVjMiU4MyU3ZSVjMiU4OHYlYzIlODklN2UlYzIlODQlYzIlODMlYzIlODglNWVZUkk=#K see SDS here] | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
*:[http:// | *:[http://labmanager.danchip.dtu.dk/d4Show.php?id=2479&mach=146 see APV here] | ||
*:[ | *:[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhERkZMSkhOSVRkJWMyJTg3JTdjdiVjMiU4MyU3ZSVjMiU4OHYlYzIlODklN2UlYzIlODQlYzIlODMlYzIlODglNWVZUkk=#K see SDS here] | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
*:[http:// | *:[http://labmanager.danchip.dtu.dk/d4Show.php?id=1897&mach=64 see APV here] | ||
*:[ | *:[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhERkVKS0lNTFRkJWMyJTg3JTdjdiVjMiU4MyU3ZSVjMiU4OHYlYzIlODklN2UlYzIlODQlYzIlODMlYzIlODglNWVZUkk=#K see SDS here] | ||
|- | |- | ||
!style="background:silver; color:black" align="center" valign="center" rowspan=" | !style="background:silver; color:black" align="center" valign="center" rowspan="3"|Performance | ||
|style="background:LightGrey; color:black"| | |style="background:LightGrey; color:black"|Isotropic | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
* | *Isotropic | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
* | *Isotropic | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
* | *Isotropic | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
* | *Isotropic | ||
|- | |- | ||
|style="background:LightGrey; color:black"|Etch rates | |style="background:LightGrey; color:black"|Etch rates | ||
[[/BHF etch rates|See more]] | |||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
* | *Wet thermal oxide:75-80nm/min | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
* | *Wet thermal oxide:~6nm/min(1%) / 25nm/min(5%) / 52nm/min(10%) | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
*Boronfloat and quartz: ~3-4 μm/min | |||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
*Thermal oxide 80 nm/min | |||
|- | |- | ||
|style="background:LightGrey; color:black"| | |style="background:LightGrey; color:black"|Lifetime of photoresist | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
* | *~½ hour | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
* | *~½ hour | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
* | *~½ hour | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
* | *~½ hour | ||
|- | |- | ||
|style="background:LightGrey; color:black"| | !style="background:silver; color:black" align="center" valign="center" rowspan="2"|Process parameter range | ||
|style="background:LightGrey; color:black"|Chemical solution | |||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
* | *BHF (12%HF with Ammoniumflouride) | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
* | *1% / 5% HF | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
* | *40% HF | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
* | *BOE 7:1 Etchant VLSI with Surfactant (BHF with a wetting agent) | ||
|- | |- | ||
|style="background:LightGrey; color:black"|Temperature | |style="background:LightGrey; color:black"|Temperature | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
* | *Room temperature | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
* | *Room temperature | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
* | *Room temperature | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
* | *Room temperature | ||
|- | |- | ||
|style="background:LightGrey; color:black"| | !style="background:silver; color:black" align="center" valign="center" rowspan="1"|Substrates | ||
|style="background:LightGrey; color:black"|Masking material | |||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
* | *Silicon nitride | ||
*Poly silicon | |||
*Photoresist | |||
*Blue film | |||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
* | *Silicon nitride | ||
*Poly silicon | |||
*Photoresist delaminates | |||
*Blue film | |||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
* | *Photoresist delaminates | ||
*Silicon nitride (Only on quartz wafers) | |||
*Poly silicon (Only on quartz wafers) | |||
*Blue film | |||
*Chromium and gold | |||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
* | *Silicon nitride | ||
*Poly silicon | |||
*Photoresist | |||
*Blue film | |||
|- | |||
|} | |||
==Life time of the photoresist and blue film in BHF== | |||
Photoresist delaminates from the substrate in BHF. For standard photoresist this process starts after about or less than ½ hour but the time can vary with resist pattern. It starts by under etching the photoresist at the edges. The life time can be prolonged a little to ½ hour - 40 minutes if the photoresist is baked at 120<sup>o</sup>C. | |||
Blue film also has a limited life time in BHF. Blue film is mainly used for back side protecting the wafer while etching on the front side. The life time of Blue film is also about ½ hour. | |||
<br clear="all" /> | |||
<gallery caption="Different places to do wet silicon oxide etch" widths="420px" heights="425px" perrow="5"> image:BHF clean.JPG|BHF in wetbench 04 in D-3 (Oxide etch 2: BHF (clean)). Wet silicon oxide etch bath positioned to the right in the wetbench. This bath can also be used for BHF with wetting agent. | |||
image:KOH_BHF.JPG|BHF in wetbench 01 Si etch in D-3 (Oxide etch 1: BHF). The BHF bath is positioned in the middle of the bench. This is primarily used to remove oxide before and after a Si etch. | |||
image:BHF clean.JPG|BHF in wetbench 05 in D-3 (Oxide etch 3: 10% HF). Wet silicon oxide etch bath positioned to the right in the wetbench. This bath can also be used for BHF, BHF with wetting agent or 40% HF on request. This bath is also used for cleaning quarts carriers from the PECVD4 system. | |||
image:RCA-HF.jpg|HF baths in RCA bench in B-1. These may only be used together with RCA cleaning and furnace processes. | |||
</gallery> | |||
<br clear="all" /> | |||
==Comparing different BHF baths== | |||
{|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" | |||
|- | |- | ||
|-style="background:silver; color:black" | |||
|style="background:WhiteSmoke; color:black"| | ! | ||
! BHF (KOH) in D-3(Oxide etch 1: BHF) | |||
| | ! BHF clean in D-3 (Oxide etch 2: BHF) | ||
! BHF in RCA Bench | |||
| | ! BHF in PP-bath | ||
! BHF Plastic beaker | |||
| | |||
|- | |||
|-style="background:WhiteSmoke; color:black" | |||
!Batch size! | |||
|1-25 wafers at a time | |||
|1-25 wafer at a time | |||
|1-25 wafers at a time | |||
|1-25 wafers at a time | |||
|1-7 wafers at a time | |||
|- | |- | ||
|style="background:LightGrey; color:black" | |||
| | |-style="background:LightGrey; color:black" | ||
!Size of substrate | |||
|2"-6" wafers | |||
| | |2"-6" wafers | ||
|2"-6" wafers | |||
| | |2"- 4" wafers or any that fits in a dedicated holder | ||
|2"- 4" wafers or any that fits in a dedicated holder | |||
| | |||
|- | |- | ||
|style="background: | |||
|-style="background:WhiteSmoke; color:black" | |||
!Allowed materials | |||
| | |||
*Silicon | *Silicon | ||
*Silicon | *Poly Silicon | ||
*Silicon | *Silicon Oxide | ||
*Silicon Nitride | |||
*Silicon Oxynitride | |||
*Photoresist | |||
*Blue film | |||
| | |||
*Silicon | *Silicon | ||
*Silicon | *Poly Silicon | ||
*Silicon | *Silicon Oxide | ||
*Silicon Nitride | |||
*Silicon Oxynitride | |||
*Photoresist | |||
*Blue film | |||
| | |||
*Silicon | *Silicon | ||
*Silicon | *Poly Silicon | ||
*Silicon ( | *Silicon Oxide | ||
|style="background:WhiteSmoke; color:black"| | *Silicon Nitride | ||
*Silicon Oxynitride | |||
| | |||
*All materials | |||
| | |||
*All materials | |||
|- | |||
|-style="background:LightGrey; color:black" | |||
!Restrictions | |||
|Wafers have to be cleaned in 7UP or RCA before further processing. | |||
|No wafers with metal are allowed in this bath | |||
|Only for wafers with phosphor glass or boron glass that comes directly from one of the furnaces in stack A. All other substrates and material are strictly forbidden to go into the tank. | |||
|None | |||
|None | |||
|- | |||
|} | |||
<br clear="all" /> | |||
==Comparing different HF baths== | |||
{|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" | |||
|- | |||
|-style="background:silver; color:black" | |||
! | |||
! 1% HF in RCA Bench | |||
! 10% HF in D3 wet bench 5 (Oxide etch 3) | |||
! 1% HF Plastic beaker | |||
|- | |||
|-style="background:WhiteSmoke; color:black" | |||
!Batch size! | |||
|1-25 wafers at a time | |||
|1-25 wafer at a time | |||
|1-7 wafers at a time | |||
|- | |||
|-style="background:LightGrey; color:black" | |||
!Size of substrate | |||
|2"-6" wafers | |||
|2"- 6" wafers or any that fits in a dedicated holder | |||
|2"- 4" wafers or any that fits in a dedicated holder | |||
|- | |||
|-style="background:WhiteSmoke; color:black" | |||
!Allowed materials | |||
|Only for wafers that are being RCA cleaned | |||
|All materials | |||
|All materials | |||
|- | |||
|} | |||
<br clear="all" /> | |||
==40% HF== | |||
{|border="1" cellspacing="1" cellpadding="2" style="text-align:left;" | |||
|- | |||
|-style="background:silver; color:black" | |||
! | |||
! 40% HF in Plastic beaker, only done by Nanolab staff | |||
|- | |||
|-style="background:WhiteSmoke; color:black" | |||
!Batch size! | |||
|1 wafer at a time | |||
|- | |||
|-style="background:LightGrey; color:black" | |||
!Size of substrate | |||
|Any that fits to a dedicated holder | |||
|- | |- | ||
| | |-style="background:WhiteSmoke; color:black" | ||
!Allowed materials | |||
|All materials | |||
| | |||
|- | |- | ||
|} | |} | ||
<br clear="all" /> | <br clear="all" /> | ||
==BOE 7:1 Etchant VLSI with Surfactant bath== | |||
{|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" | |||
|- | |||
|-style="background:silver; color:black" | |||
! | |||
! BOE 7:1 Etchant VLSI with Surfactant bath | |||
|- | |||
|-style="background:WhiteSmoke; color:black" | |||
!Batch size! | |||
|1-25 wafers at a time | |||
|- | |||
|-style="background:LightGrey; color:black" | |||
!Size of substrate | |||
|4" wafers | |||
|- | |||
|-style="background:WhiteSmoke; color:black" | |||
!Allowed materials | |||
| | |||
*Silicon | |||
*Poly silicon | |||
*Silicon nitrides | |||
*Silicon oxynitrides | |||
*Silicon oxides | |||
*Photoresist | |||
|- | |||
|-style="background:WhiteSmoke; color:black" | |||
!Remark | |||
| | |||
Amorphous silicon can be used as a mask fro SiO2 etching.<br/> | |||
For very long and deep etches of SiO2/Quartz (several hours/micrometers) <br/> | |||
we have indications that show that it is not good to use the BOE 7:1 Etchant VLSI with Surfactant etch. <br/> | |||
The amorphous silicon has small holes (etch pits) which the BOE 7:1 Etchant VLSI with Surfactant etch penetrates and the SiO2 below is etched. | |||
|- | |||
|} | |||
Latest revision as of 14:31, 15 September 2026
Feedback to this page: click here
Unless anything else is stated, everything on this page, text and pictures are made by DTU Nanolab.
All links to Kemibrug (SDS) and Labmanager Including APV, requires login.
Etch Wet Silicon Oxide Silicon Oxide
Wet Silicon Oxide Etch (BHF, HF and BOE 7:1 Etchant VLSI)
Silicon oxide can be etched using HF. At DTU Nanolab it is mainly used in a buffered version BHF (premixed). You can find safety datasheets on Kemibrug here The BHF has a stable etch rate and is gentle to photoresist due to an almost pH neutral solution which makes photoresist a good masking material for the oxide etch.
BOE 7:1 Etchant VLSI with Surfactant (BHF with wetting agent) can also be used for etching silicon oxide. This is mainly for etching small holes. At DTU Nanolab we do not have BHF with wetting agent in a prepared bath, it's only to be used in fumehoods. It's not very often used and we do not have it as a standard chemical. Please contact DTU Nanolab if you need it.
Wafers with metals or other materials, not allowed in the dedicated oxide etch baths, can be etched using a plastic beaker in Fume hood 01 or 02 (Acids/bases) in D-3. Samples with III-V materials (e.g. InP and GaAs) must be etched in Fume hood 07: III-V Avids/bases in D-3.
The user manual for Oxide etch 1: BHF, APV's and contact information can be found in LabManager by clicking here
The user manual for Oxide etch 2: BHF (clean), APV's and contact information can be found in LabManager by clicking here
The user manual for Oxide etch 3: 10% HF, APV's and contact information can be found in LabManager by clicking here
The user manual for various HF baths in RCA and Fume hoods, APV's and contact information can be found in LabManager by clicking here
Working with HF above 13% is only allowed by Nanolab staff
Process information:
See more etch rates in HF solutions.
| Etchant | BHF | 1% HF / 5% HF / 10% HF | 40% HF | BOE 7:1 Etchant VLSI with Surfactant | |
|---|---|---|---|---|---|
| Purpose | Etching of silicon oxide |
|
|
|
|
| Link to safety APV and SDS (You must be logged in to Kemibrug to view SDSs) | |||||
| Performance | Isotropic |
|
|
|
|
| Etch rates |
|
|
|
| |
| Lifetime of photoresist |
|
|
|
| |
| Process parameter range | Chemical solution |
|
|
|
|
| Temperature |
|
|
|
| |
| Substrates | Masking material |
|
|
|
|
Life time of the photoresist and blue film in BHF
Photoresist delaminates from the substrate in BHF. For standard photoresist this process starts after about or less than ½ hour but the time can vary with resist pattern. It starts by under etching the photoresist at the edges. The life time can be prolonged a little to ½ hour - 40 minutes if the photoresist is baked at 120oC.
Blue film also has a limited life time in BHF. Blue film is mainly used for back side protecting the wafer while etching on the front side. The life time of Blue film is also about ½ hour.
- Different places to do wet silicon oxide etch
-
BHF in wetbench 04 in D-3 (Oxide etch 2: BHF (clean)). Wet silicon oxide etch bath positioned to the right in the wetbench. This bath can also be used for BHF with wetting agent.
-
BHF in wetbench 01 Si etch in D-3 (Oxide etch 1: BHF). The BHF bath is positioned in the middle of the bench. This is primarily used to remove oxide before and after a Si etch.
-
BHF in wetbench 05 in D-3 (Oxide etch 3: 10% HF). Wet silicon oxide etch bath positioned to the right in the wetbench. This bath can also be used for BHF, BHF with wetting agent or 40% HF on request. This bath is also used for cleaning quarts carriers from the PECVD4 system.
-
HF baths in RCA bench in B-1. These may only be used together with RCA cleaning and furnace processes.
Comparing different BHF baths
| BHF (KOH) in D-3(Oxide etch 1: BHF) | BHF clean in D-3 (Oxide etch 2: BHF) | BHF in RCA Bench | BHF in PP-bath | BHF Plastic beaker | |
|---|---|---|---|---|---|
| Batch size! | 1-25 wafers at a time | 1-25 wafer at a time | 1-25 wafers at a time | 1-25 wafers at a time | 1-7 wafers at a time |
| Size of substrate | 2"-6" wafers | 2"-6" wafers | 2"-6" wafers | 2"- 4" wafers or any that fits in a dedicated holder | 2"- 4" wafers or any that fits in a dedicated holder |
| Allowed materials |
|
|
|
|
|
| Restrictions | Wafers have to be cleaned in 7UP or RCA before further processing. | No wafers with metal are allowed in this bath | Only for wafers with phosphor glass or boron glass that comes directly from one of the furnaces in stack A. All other substrates and material are strictly forbidden to go into the tank. | None | None |
Comparing different HF baths
| 1% HF in RCA Bench | 10% HF in D3 wet bench 5 (Oxide etch 3) | 1% HF Plastic beaker | |
|---|---|---|---|
| Batch size! | 1-25 wafers at a time | 1-25 wafer at a time | 1-7 wafers at a time |
| Size of substrate | 2"-6" wafers | 2"- 6" wafers or any that fits in a dedicated holder | 2"- 4" wafers or any that fits in a dedicated holder |
| Allowed materials | Only for wafers that are being RCA cleaned | All materials | All materials |
40% HF
| 40% HF in Plastic beaker, only done by Nanolab staff | |
|---|---|
| Batch size! | 1 wafer at a time |
| Size of substrate | Any that fits to a dedicated holder |
| Allowed materials | All materials |
BOE 7:1 Etchant VLSI with Surfactant bath
| BOE 7:1 Etchant VLSI with Surfactant bath | |
|---|---|
| Batch size! | 1-25 wafers at a time |
| Size of substrate | 4" wafers |
| Allowed materials |
|
| Remark |
Amorphous silicon can be used as a mask fro SiO2 etching. |