Jump to content

Specific Process Knowledge/Etch/Wet Chromium Etch: Difference between revisions

From LabAdviser
Choi (talk | contribs)
Mbec (talk | contribs)
 
(14 intermediate revisions by 5 users not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:wetchemistry@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Etch/Wet_Chrominum_Etch click here]'''
'''Feedback to this page''': '''[mailto:wetchemistry@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/Wet_Chrominum_Etch click here]'''
 
'''Unless anything else is stated, everything on this page, text and pictures are made by DTU Nanolab.'''
 
'''All links to Kemibrug (SDS) and Labmanager Including APV requires login.'''
 
'''All measurements on this page has been made by Nanolab staff.'''  


[[Category: Equipment|Etch Wet Chromium]]
[[Category: Etch (Wet) bath|Chromium]]


==Wet etching of Chromium==
==Wet etching of Chromium==
[[Image:Fumehood1-2.jpg|300x300px|thumb|Fume hood 01 or 02 (for acids and bases) in cleanroom D-3 can be used for wet chromium etching.]]
[[File:Si etch 3.png|300x300px |thumb| Work space in Fume Hood 06 in cleanroom D-3 can be used for wet chromium etching - workspace should be booked.]]
Wet etching of chromium at Danchip is done making your own set up in a beaker in a fume hood - preferably in D-3. You can see the APV [http://labmanager.dtu.dk/d4Show.php?id=4748&mach=368 here].


We use the following solution to etch chromium:
We use the following solution to etch chromium:


# Commercial chromium etch (Chrome Etch 18). You can see the KBA [http://kemibrug.dk/KBA/CAS/107388/?show_KBA=1&portaldesign=1 here]
# Commercial chromium etch (Chrome Etch 18). You can see the KBA (needs login to kemibrug) [https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhESk5HTklNVGQlYzIlODclN2N2JWMyJTgzJTdlJWMyJTg4diVjMiU4OSU3ZSVjMiU4NCVjMiU4MyVjMiU4OCU1ZVlSSQ==#K here]
 
The etch rate depends on the level of surface oxidation of the chromium metal, but the standard procedure (etch at room temperature: ~22°C) the Etch rate is around 150 nm/min.
 
'''Etch in Fume hood'''
Wet etching of chromium in fume hood at DTU Nanolab is done making your own set up in a beaker in a fume hood - preferably fume hood 6 for Si etch 3 in D-3
 
You can see the APV [https://labmanager.dtu.dk/d4mb/show.php?dokId=4748&mach=368&chpr=0 here].
 
PECVD SiO2 and LPCVD SiN coated wafers have been immersed in Cr etch 18 for 10min. Thickness wise: absolutely no changes (roughness after etch not measured)
 
Normally the etch is reused (if you etch Molybdenum never reuse), but if you need to dispose it, collect it in a bottle marked X waste.
 
'''Etching of Chromium in Acid 1 wetbench 11'''
[[File:Wetbench 11.png|300x300px|thumb|Acid 1 Wetbench 11 in cleanroom D-3 can be used for wet chromium etching of 6" and 8" wafers, after agreement with wetchemistry group.]]
 
Always make an agreement with Wetchemistry group before training


The etch rate depends on the level of surface oxidation of the chromium metal, but the standard procedure (etch at room temperature: ~22°C) the etch rate is around 150 nm/min.
The bath is for 6" and 8" wafers.
 
You can see the APV [https://labmanager.dtu.dk/d4mb/show.php?dokId=21726&mach=580 here].


===Overview of the chromium etch process===
===Overview of the chromium etch process===
Line 21: Line 42:
|-style="background:silver; color:black"
|-style="background:silver; color:black"
!
!
! Chromium etch 1
! Chromium etch in Fume hood
! Chromium etch Acid 1 wetbench 11
|-  
|-  


Line 28: Line 50:
|
|
Etch of chromium
Etch of chromium
|
Etch of Chromium 6" and 8" wafers 
|-
|-


Line 33: Line 57:
!Link to safety APV and KBA
!Link to safety APV and KBA
|[http://labmanager.dtu.dk/d4Show.php?id=4748&mach=368 see fumehood APV/manual here].  
|[http://labmanager.dtu.dk/d4Show.php?id=4748&mach=368 see fumehood APV/manual here].  
[http://kemibrug.dk/KBA/CAS/107388/?show_KBA=1&portaldesign=1 see Chrome Etch 18 KBA here]
[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhESk5HTklNVGQlYzIlODclN2N2JWMyJTgzJTdlJWMyJTg4diVjMiU4OSU3ZSVjMiU4NCVjMiU4MyVjMiU4OCU1ZVlSSQ==#K see Chrome Etch 18 KBA here]
|[https://labmanager.dtu.dk/d4mb/show.php?dokId=21726&mach=580 see Wetbench 11 APV/manual here].
[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhESk5HTklNVGQlYzIlODclN2N2JWMyJTgzJTdlJWMyJTg4diVjMiU4OSU3ZSVjMiU4NCVjMiU4MyVjMiU4OCU1ZVlSSQ==#K see Chrome Etch 18 KBA here]
|-
|-


|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
!Chemical solution
!Chemical solution
|Chrome Etch 18
|Chrome Etch 18
|Chrome Etch 18
|-
|-
Line 44: Line 71:
!Process temperature
!Process temperature
|Room temperature
|Room temperature
 
|Room temperature
|-
|-


|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
!Possible masking materials
!Possible masking materials
|Photoresist (1.5 µm AZ5214E)
|Photoresist (1.5 µm AZ5214E)
|Photoresist (1.5 µm AZ5214E)
|-
|-
Line 54: Line 82:
|-style="background:LightGrey; color:black"
|-style="background:LightGrey; color:black"
!Etch rate
!Etch rate
|~ 150 nm/min at 22°C
|~ 150 nm/min at 22°C
|~ 150 nm/min at 22°C
|-
|-
Line 60: Line 89:
!Batch size
!Batch size
|1-7 4" wafers at a time
|1-7 4" wafers at a time
|Up to 5 6" or 8" wafers at a time
|-
|-


|-style="background:LightGrey; color:black"
|-style="background:LightGrey; color:black"
!Size of substrate
!Size of substrate
|Any size and number that can go inside the beaker in use
|Any size and number that can go inside the beaker in use
|6" and 8" 
|-
|-


Line 71: Line 102:
|No restrictions.  
|No restrictions.  
Make a note on the beaker of which materials have been processed.
Make a note on the beaker of which materials have been processed.
|
See the [https://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=580 Cross Contamination Sheet] for Acid 1
|-
|-
|}
|}

Latest revision as of 11:57, 30 June 2026

Feedback to this page: click here

Unless anything else is stated, everything on this page, text and pictures are made by DTU Nanolab.

All links to Kemibrug (SDS) and Labmanager Including APV requires login.

All measurements on this page has been made by Nanolab staff.


Wet etching of Chromium

Work space in Fume Hood 06 in cleanroom D-3 can be used for wet chromium etching - workspace should be booked.

We use the following solution to etch chromium:

  1. Commercial chromium etch (Chrome Etch 18). You can see the KBA (needs login to kemibrug) here

The etch rate depends on the level of surface oxidation of the chromium metal, but the standard procedure (etch at room temperature: ~22°C) the Etch rate is around 150 nm/min.

Etch in Fume hood Wet etching of chromium in fume hood at DTU Nanolab is done making your own set up in a beaker in a fume hood - preferably fume hood 6 for Si etch 3 in D-3

You can see the APV here.

PECVD SiO2 and LPCVD SiN coated wafers have been immersed in Cr etch 18 for 10min. Thickness wise: absolutely no changes (roughness after etch not measured)

Normally the etch is reused (if you etch Molybdenum never reuse), but if you need to dispose it, collect it in a bottle marked X waste.

Etching of Chromium in Acid 1 wetbench 11

Acid 1 Wetbench 11 in cleanroom D-3 can be used for wet chromium etching of 6" and 8" wafers, after agreement with wetchemistry group.

Always make an agreement with Wetchemistry group before training

The bath is for 6" and 8" wafers.

You can see the APV here.

Overview of the chromium etch process

Chromium etch in Fume hood Chromium etch Acid 1 wetbench 11
General description

Etch of chromium

Etch of Chromium 6" and 8" wafers

Link to safety APV and KBA see fumehood APV/manual here.

see Chrome Etch 18 KBA here

see Wetbench 11 APV/manual here.

see Chrome Etch 18 KBA here

Chemical solution Chrome Etch 18 Chrome Etch 18
Process temperature Room temperature Room temperature
Possible masking materials Photoresist (1.5 µm AZ5214E) Photoresist (1.5 µm AZ5214E)
Etch rate ~ 150 nm/min at 22°C ~ 150 nm/min at 22°C
Batch size 1-7 4" wafers at a time Up to 5 6" or 8" wafers at a time
Size of substrate Any size and number that can go inside the beaker in use 6" and 8"
Allowed materials No restrictions.

Make a note on the beaker of which materials have been processed.

See the Cross Contamination Sheet for Acid 1