| (18 intermediate revisions by the same user not shown) |
| Line 8: |
Line 8: |
| __TOC__ | | __TOC__ |
|
| |
|
| =Plasma Asher 1= | | = Descum Comparison Table = |
| <span style="color:red">Plasma asher 1 was decommissioned 2024-12-02.</span>
| |
| | |
| [[Specific Process Knowledge/Lithography/Descum/PlasmaAsher1|Information about decommissioned tool can be found here.]]
| |
| <br clear="all" />
| |
| | |
| =Plasma Asher 2=
| |
| <span style="color:red">Plasma asher 2 was decommissioned 2024-12-02.</span>
| |
| | |
| [[Specific Process Knowledge/Lithography/Descum/PlasmaAsher2|Information about decommissioned tool can be found here.]]
| |
| <br clear="all" />
| |
| | |
| =Plasma Asher 3: Descum=
| |
| The user manual(s), quality control procedure(s) and results and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=423 LabManager] - '''requires login'''
| |
| | |
| Plasma Asher 3 is specifically used for controlled descum process after lithography. Please note that you only can process a single 100 mm wafer, or one small sample, at a time.
| |
| The plasma asher is equipped with 2 gaslines: oxygen and nitrogen, but all standard processes use only oxygen (as recommended by Diener).
| |
| | |
| '''Process parameters'''<br>
| |
| You can manipulate two different descum process development parameters: you can either change power or chamber pressure.
| |
| | |
| ==Power testing - AZ MiR 701==
| |
| [[image:AZMIR701_power_settings.png|400px|thumb|Descum results for different power settings]]
| |
| | |
| '''Recipe settings:'''
| |
| *Resist: AZ MiR 701
| |
| *O2 flow: 5 sccm
| |
| *N2 flow: 0
| |
| *Pressure: 0.2 mbar
| |
| *Power: Varied
| |
| | |
| {| class="wikitable" style="text-align: center;"
| |
| |+ style="caption-side: top; text-align: left;" | Experiment parameters
| |
| |-
| |
| ! !! Forward/reverse !! C2/C1 !! Power
| |
| |-
| |
| | style="text-align: left;" | '''recipe 1''' || 50/0 || 52/31 || 50%
| |
| |-
| |
| | style="text-align: left;" | '''recipe 2''' || 100/0 || 53/31 || 100%
| |
| |-
| |
| | style="text-align: left;" | '''recipe 3''' || 20/0 || 51/34 || 20%
| |
| |}
| |
| | |
| ==Pressure testing - AZ MiR 701==
| |
| [[image:AZMIR701_pressure_settings.png|400px|thumb|Descum results for different pressure settings]]
| |
| | |
| '''Recipe settings:'''
| |
| *Resist: AZ MiR 701
| |
| *O2 flow: varied
| |
| *N2 flow: 0
| |
| *Pressure: varied
| |
| *Power: V100% (100 W)
| |
| | |
| {| class="wikitable" style="text-align: center;"
| |
| |+ style="caption-side: top; text-align: left;" | Experiment parameters
| |
| |-
| |
| ! !! Forward/reverse !! C2/C1 !! Oxygen !! Pressure
| |
| |-
| |
| | style="text-align: left;" | '''recipe 1''' || 100/0 || 52/31 || 5 || 0.2
| |
| |-
| |
| | style="text-align: left;" | '''recipe 2''' || 100/0 || 37/38 || 45 || 0.8
| |
| |}
| |
| | |
| ==Pressure testing - AZ 5214E==
| |
| [[image:AZ5214E_pressure_settings.png|400px|thumb|Descum results for different pressure settings]]
| |
| | |
| '''Recipe settings:'''
| |
| *Resist: AZ 5214E
| |
| *O2 flow: varied
| |
| *N2 flow: 0
| |
| *Pressure: varied
| |
| *Power: V100% (100 W)
| |
| | |
| {| class="wikitable" style="text-align: center;"
| |
| |+ style="caption-side: top; text-align: left;" | Experiment parameters
| |
| |-
| |
| ! !! Forward/reverse !! C2/C1 !! Oxygen !! Pressure
| |
| |-
| |
| | style="text-align: left;" | '''recipe 1''' || 100/0 || 52/31 || 17 || 0.4
| |
| |-
| |
| | style="text-align: left;" | '''recipe 2''' || 100/0 || 37/39 || 45 || 0.8
| |
| |}
| |
| | |
| <br clear="all" />
| |
| | |
| =Plasma Asher 4=
| |
| Descum of AZ 5214E on 100 mm wafers. The descum process development was done for a single substrate, as well as 3 substrates (for decreased ashing rate and improved ashing uniformity). The substrates were placed vertically in the glass boat. | |
| | |
| <gallery style="text-align: center;" widths=250 heights=250>
| |
| PA_boat_1Wafer_v2.png|Single vertical substrate
| |
| PA_boat_3Wafer_v2.png|3 vertical substrates - dummy/test wafer/dummy
| |
| </gallery>
| |
| | |
| For the 3 substrates only the center substrate was used for testing, the front and back wafers were used as dummy wafers. The wafers were placed in consecutive slots - when running multiple wafers in this way, the first and last wafers should always be dummy wafers.
| |
| | |
| The user manual, risk assessment, and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=530 LabManager] - '''requires login'''
| |
| | |
| '''Typical descum parameters'''<br>
| |
| Tested with 1.5 µm AZ 5214E on 100 mm silicon substrate.
| |
| *O<sub>2</sub>: 100 sccm
| |
| *N<sub>2</sub>: 100 sccm
| |
| *Pressure (DSC): 1.3 mbar
| |
| *Power: 200 W
| |
| *Chamber temperature at start (with door closed): 30°C
| |
| *Time (single wafer): 5-10 minutes = 35-72 nm ashed
| |
| *Time (multiple wafers): 10-15 minutes = 40-80 nm ashed
| |
| | |
| {| class="wikitable" | | {| class="wikitable" |
| |- | | |- |
| ! Test setup !! Single substrate !! Center of 3 substrates | | ! |
| |-
| | ! [[Specific_Process_Knowledge/Lithography/Descum/plasmaAsher03|Plasma Asher 3: Descum]] |
| ! scope=row| Test results | | ! [[Specific_Process_Knowledge/Lithography/Descum/plasmaAsher04|Plasma Asher 4 (Clean)]] |
| | Ashing rate: 5.7 ±2.1 nm/min<br>Non-uniformity: 0.6 ±0.4% || Ashing rate: 3.8 ±1.6 nm/min<br>Non-uniformity: 0.4 ±0.2%
| | ! [[Specific_Process_Knowledge/Lithography/Descum/plasmaAsher05|Plasma Asher 5 (Dirty)]] |
| |-
| |
| ! scope=row| Wafers | |
| | 1 || 3
| |
| |-
| |
| ! scope=row| Wafer size | |
| | 100 mm || 100 mm
| |
| |-
| |
| ! scope=row| Boat position
| |
| | Center of chamber || Center of chamber
| |
| |-
| |
| ! scope=row| Test wafer position
| |
| | Center of boat || Center of boat
| |
| |- | | |- |
| ! scope=row| Total gas flow rate | | ! scope=row style="text-align: left;" | Purpose |
| | 200 sccm || 200 sccm | | | Resist descum |
| | | |
| | *Resist stripping |
| | *Resist descum |
| | | |
| | *Resist stripping |
| | *Resist descum |
| |- | | |- |
| ! scope=row| Gas mix ratio | | ! scope=row style="text-align: left;" | Method |
| | 50% N<sub>2</sub> || 50% N<sub>2</sub> | | | Plasma ashing |
| | | Plasma ashing |
| | | Plasma ashing |
| |- | | |- |
| ! scope=row| Chamber pressure | | ! scope=row style="text-align: left;" | Process gasses |
| | 1.3 mbar || 1.3 mbar | | | O<sub>2</sub> (50 sccm) |
| | | |
| | *O<sub>2</sub> (0-500 sccm) |
| | *N<sub>2</sub> (0-500 sccm) |
| | | |
| | *O<sub>2</sub> (0-500 sccm) |
| | *N<sub>2</sub> (0-500 sccm) |
| | *CF<sub>4</sub> (0-200 sccm) |
| |- | | |- |
| ! scope=row| Power | | ! scope=row style="text-align: left;" | Process power |
| | 200 W || 200 W | | | 10-100 W (10-100%) |
| | | 150-1000 W |
| | | 150-1000 W |
| |- | | |- |
| ! scope=row| Test processing time | | ! scope=row style="text-align: left;" | Substrate batch |
| | Tested parameter || Tested parameter | | | |
| | *Chips: several |
| | *50 mm wafer: several |
| | *100 mm wafer: 1 |
| | | |
| | *Chips: several |
| | *50 mm wafer: several |
| | *100 mm wafer: 1-25 |
| | *150 mm wafer: 1-25 |
| | *200 mm wafer: 1-25 |
| | | |
| | *Chips: several |
| | *50 mm wafer: several |
| | *100 mm wafer: 1-25 |
| | *150 mm wafer: 1-25 |
| | *200 mm wafer: 1-25 |
| |- | | |- |
| ! scope=row| Test average temperature | | ! scope=row style="text-align: left;" | Substrate materials |
| | 33°C || 33°C | | | |
| | *<span style="color:red">'''No polymer substrates'''</span><br> |
| | *Silicon substrates |
| | *III-V substrates |
| | *Glass substrates |
| | *Films, or patterned films, of any material except type IV (Pb, Te) |
| | | |
| | *<span style="color:red">'''No metals'''</span><br> |
| | *<span style="color:red">'''No metal oxides'''</span><br> |
| | *<span style="color:red">'''No III-V materials'''</span><br> |
| | *Silicon substrates |
| | *Glass substrates |
| | *Polymer substrates |
| | *Films, or patterned films, of resists/polymers |
| | | |
| | *Silicon substrates |
| | *III-V substrates |
| | *Glass substrates |
| | *Polymer substrates |
| | *Films, or patterned films, of any material except type IV (Pb, Te) |
| |} | | |} |
|
| |
|
| <br clear="all" /> | | =Decommisioned tools= |
| | <span style="color:red">Plasma asher 1 was decommissioned 2024-12-02.</span> |
|
| |
|
| ==Single wafer descum ashing rate and uniformity for plasma asher 4 & 5==
| | [[Specific Process Knowledge/Lithography/Descum/PlasmaAsher1|Information about decommissioned tool can be found here.]] |
| [[File:PA_descum_single_v3.png|400px|thumb|Ashing amount and ashing rate when processing a single 100 mm wafer.|right]] | |
|
| |
|
| {| class="wikitable" style="text-align: center;"
| |
| |+ style="caption-side: top; text-align: left;" | Ashing amount and rate
| |
| |-
| |
| ! style="text-align: left;" | Ashing time [min]: !! 1 !! 2 !! 5 !! 10 !! 15
| |
| |-
| |
| | style="text-align: left;" | Ashing amount [nm]: || 5.2 || 6.2 || 35.1 || 72.3 || 87.1
| |
| |-
| |
| | style="text-align: left;" | Ashing rate [nm/min]: || 5.2 || 3.1 || 7.0 || 7.2 || 5.8
| |
| |}
| |
|
| |
|
| {| class="wikitable" style="text-align: center;"
| | <span style="color:red">Plasma asher 2 was decommissioned 2024-12-02.</span> |
| |+ style="caption-side: top; text-align: left;" | Ashing non-uniformity
| |
| |-
| |
| ! style="text-align: left;" | Ashing time [min]: !! 1 !! 2 !! 5 !! 10 !! 15
| |
| |-
| |
| | style="text-align: left;" | Pre-descum film thickness range [nm]: || 11 || 12 || 10 || 11 || 9
| |
| |-
| |
| | style="text-align: left;" | Pre-descum non-uniformity [%]: || 0.37 || 0.40 || 0.33 || 0.37 || 0.30
| |
| |-
| |
| | style="text-align: left;" | Post-descum film thickness range [nm]: || 10 || 10 || 12 || 19 || 33
| |
| |-
| |
| | style="text-align: left;" | Post-descum non-uniformity [%]: || 0.33 || 0.33 || 0.41 || 0.66 || 1.18
| |
| |}
| |
| | |
| <br clear="all" /> | |
| | |
| ==Multi wafer descum ashing rate and uniformity for plasma asher 4 & 5==
| |
| [[File:PA_descum_multi_v3.png|400px|thumb|Ashing amount and ashing rate when processing multiple 100 mm wafers. Test measured on the center of 3 wafers.|right]]
| |
| | |
| {| class="wikitable" style="text-align: center;"
| |
| |+ style="caption-side: top; text-align: left;" | Ashing amount and rate
| |
| |-
| |
| ! style="text-align: left;" | Ashing time [min]: !! 1 !! 2 !! 5 !! 10 !! 15
| |
| |-
| |
| | style="text-align: left;" | Ashing amount [nm]: || 4.3 || 6.7 || 10.1 || 39.5 || 78.8
| |
| |-
| |
| | style="text-align: left;" | Ashing rate [nm/min]: || 4.3 || 3.4 || 2.0 || 4.0 || 5.3
| |
| |}
| |
| | |
| {| class="wikitable" style="text-align: center;"
| |
| |+ style="caption-side: top; text-align: left;" | Ashing non-uniformity
| |
| |-
| |
| ! style="text-align: left;" | Ashing time [min]: !! 1 !! 2 !! 5 !! 10 !! 15
| |
| |-
| |
| | style="text-align: left;" | Pre-descum film thickness range [nm]: || 11 || 13 || 11 || 12 || 14
| |
| |-
| |
| | style="text-align: left;" | Pre-descum non-uniformity [%]: || 0.37 || 0.43 || 0.37 || 0.40 || 0.46
| |
| |-
| |
| | style="text-align: left;" | Post-descum film thickness range [nm]: || 11 || 9 || 10 || 12 || 21
| |
| |-
| |
| | style="text-align: left;" | Post-descum non-uniformity [%]: || 0.37 || 0.30 || 0.33 || 0.41 || 0.74
| |
| |}
| |
|
| |
|
| | [[Specific Process Knowledge/Lithography/Descum/PlasmaAsher2|Information about decommissioned tool can be found here.]] |
| <br clear="all" /> | | <br clear="all" /> |
|
| |
| ==Comparison between single substrate processing and multi substrate processing for plasma asher 4 & 5==
| |
| Processing a single substrate using the standard descum settings will provide users with a relatively controllable and uniform process. Adding dummy substrates in close proximity with the process substrate will reduce the ashing rate and improve the uniformity:
| |
| <gallery mode="packed-hover" heights="150">
| |
| PA_descum_compareAmount_v1.png|Ashing amount
| |
| PA_descum_compareRate_v1.png|Ashing rate
| |
| PA_descum_compareUniformity_v1.png|Non-uniformity
| |
| </gallery>
| |
|
| |
| <br clear="all" />
| |
|
| |
| =Plasma Asher 5=
| |
| Plasma asher 5 is identical to plasma asher 4, see descum processing for plasma asher 4 [[Specific_Process_Knowledge/Lithography/Descum#Plasma_Asher_4|here]].
| |