==Descum | '''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Lithography/Descum click here]''' | ||
[[Category: Equipment|Lithography descum]] | |||
[[Category: Lithography|Descum]] | |||
__TOC__ | |||
= Descum Comparison Table = | |||
Descum | {| class="wikitable" | ||
|- | |||
! | |||
! [[Specific_Process_Knowledge/Lithography/Descum/plasmaAsher03|Plasma Asher 3: Descum]] | |||
! [[Specific_Process_Knowledge/Lithography/Descum/plasmaAsher04|Plasma Asher 4 (Clean)]] | |||
| | ! [[Specific_Process_Knowledge/Lithography/Descum/plasmaAsher05|Plasma Asher 5 (Dirty)]] | ||
! | |||
! | |||
|- | |- | ||
! scope=row style="text-align: left;" | Purpose | |||
| Resist descum | |||
| | | | ||
|| | *Resist stripping | ||
*Resist descum | |||
| | |||
*Resist stripping | |||
*Resist descum | |||
|- | |- | ||
| | ! scope=row style="text-align: left;" | Method | ||
| Plasma ashing | |||
| Plasma ashing | |||
| Plasma ashing | |||
|- | |- | ||
| 2 || 500 | ! scope=row style="text-align: left;" | Process gasses | ||
| O<sub>2</sub> (50 sccm) | |||
| | |||
*O<sub>2</sub> (0-500 sccm) | |||
*N<sub>2</sub> (0-500 sccm) | |||
| | |||
*O<sub>2</sub> (0-500 sccm) | |||
*N<sub>2</sub> (0-500 sccm) | |||
*CF<sub>4</sub> (0-200 sccm) | |||
|- | |- | ||
! scope=row style="text-align: left;" | Process power | |||
| 10-100 W (10-100%) | |||
| 150-1000 W | |||
| 150-1000 W | |||
|- | |||
|- | |||
|- | |- | ||
| | ! scope=row style="text-align: left;" | Substrate batch | ||
| | |||
*Chips: several | |||
*50 mm wafer: several | |||
*100 mm wafer: 1 | |||
| | |||
*Chips: several | |||
*50 mm wafer: several | |||
*100 mm wafer: 1-25 | |||
*150 mm wafer: 1-25 | |||
*200 mm wafer: 1-25 | |||
| | |||
*Chips: several | |||
*50 mm wafer: several | |||
*100 mm wafer: 1-25 | |||
*150 mm wafer: 1-25 | |||
*200 mm wafer: 1-25 | |||
|- | |- | ||
! scope=row style="text-align: left;" | Substrate materials | |||
| | |||
*<span style="color:red">'''No polymer substrates'''</span><br> | |||
*Silicon substrates | |||
*III-V substrates | |||
*Glass substrates | |||
*Films, or patterned films, of any material except type IV (Pb, Te) | |||
| | |||
*<span style="color:red">'''No metals'''</span><br> | |||
*<span style="color:red">'''No metal oxides'''</span><br> | |||
*<span style="color:red">'''No III-V materials'''</span><br> | |||
*Silicon substrates | |||
*Glass substrates | |||
*Polymer substrates | |||
*Films, or patterned films, of resists/polymers | |||
| | |||
*Silicon substrates | |||
*III-V substrates | |||
*Glass substrates | |||
*Polymer substrates | |||
*Films, or patterned films, of any material except type IV (Pb, Te) | |||
|} | |} | ||
=Decommisioned tools= | |||
<span style="color:red">Plasma asher 1 was decommissioned 2024-12-02.</span> | |||
[[Specific Process Knowledge/Lithography/Descum/PlasmaAsher1|Information about decommissioned tool can be found here.]] | |||
<span style="color:red">Plasma asher 2 was decommissioned 2024-12-02.</span> | |||
[[Specific Process Knowledge/Lithography/Descum/PlasmaAsher2|Information about decommissioned tool can be found here.]] | |||
<br clear="all" /> | |||