Jump to content

Specific Process Knowledge/Lithography/UVLithography: Difference between revisions

From LabAdviser
Taran (talk | contribs)
Taran (talk | contribs)
 
(33 intermediate revisions by 3 users not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/UVLithography click here]'''
{{cc-nanolab}}


[[Image:UVLithography.jpg|320x320px|right|frame|]]
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Lithography/UVLithography click here]'''


UV Lithography uses ultraviolet light to transfer a pattern from a photo-mask or a design file to a wafer coated with photoresist. The photoresist film is spin coated onto the wafers, the design is transferred to the resist by using an aligner, and subsequently the resist pattern is developed. DTU Nanolab houses a number of automatic or manual coaters, mask or maskless aligners, as well as automatic or semi-automatic developers.
[[Category: Equipment|Lithography]]
[[Category: Lithography]]


= Getting started =
[[Image:UVLithography.jpg|400px|right|]]


[[File:UVLPic1.png|450px|right]]
__TOC__


[[File:UVLPic2.png|160px|right]]
=UV lithography=
UV Lithography uses ultraviolet light to transfer a pattern from a photo-mask, or a digital design file, to a substrate coated with photoresist.  


'''Before you plan your UV processing and request for training on any equipment in UV lithography, please go through the following steps.''' Include the information in the training request.
The process has 3 main steps:
# Coating the substrate with a photosensitive film
# Transferring a pattern into the resist by exposing it with UV light through either a physical shadow mask or a digital version of a shadow mask
# Developing the exposed resist to reveal the transferred pattern


Also, please remember that the [[LabAdviser/Courses/TPT_Lithography|'''Lithography Tool Package Training''']] is mandatory before training in any lithography equipment.
DTU Nanolab offers a number of automatic and manual coaters, mask or maskless exposure tools, as well as automatic or semi-automatic developers.<br clear=all />


If you are new to photolithography, you can visit <u>[https://en.wikipedia.org/wiki/Photolithography this]</u> wikipedia webpage about photolithography before you start.
=Getting started with UV lithography=
<br> <br>


* '''Complete the TPT Lithography course''': [[LabAdviser/Courses/TPT_Lithography|Lithography Tool Package Training]].
[[File:UVLPic1.png|450px|right]]


* '''Prepare a process flow''' which describes all steps in your UV lithography process. You can find docx-templates <u>[[Specific_Process_Knowledge/Lithography/UVLithography#Resist_Overview|in this table]]</u>.
[[File:UVLPic2.png|160px|right]]


* '''Design device''': Design your device and layout. A detailed instruction on how to design a layout (mask) can be found <u>[[Specific_Process_Knowledge/Pattern_Design|here]]</u>.
<span style="color:red">New users are always recommended to have their process evaluated by the fabrication support group - before you start planning your UV process, and request training on UV lithography equipment, please go through the following pre-cleanroom and cleanroom steps and include all the information in your request.</span>  


* '''Substrate pretreatment''': In many processes it is recommended to <u>[[Specific_Process_Knowledge/Lithography/Pretreatment|pretreat or prime]]</u> your wafer before spin-coating. In some <u>[[Specific_Process_Knowledge/Lithography/Coaters|spin-coaters]]</u>, these pretreatment processes are included in the spin coating of resist.  
Please remember that the [https://labadviser.nanolab.dtu.dk//index.php?title=Specific_Process_Knowledge/Lithography#Lithography_Tool_Package_Training Lithography TPT] is <i>mandatory</i> before you can receive training on any lithography equipment.<br>
If you are completely new to photolithography, you can visit <u>[https://en.wikipedia.org/wiki/Photolithography this]</u> wikipedia webpage about photolithography before you start.


* '''Resist Type''': Choose the type of resist you wish to use: a list of UV lithography resist types available at DTU Nanolab can be found <u>[[Specific_Process_Knowledge/Lithography/UVLithography#Resist_Overview|on this page]]</u>.
** Positive tone resist: Resist exposed to UV light will be dissolved in the developer. The mask openings are an exact copy of the resist pattern which is to remain on the wafer.
** Negative tone resist: Resist exposed to UV light will become polymerized and difficult to dissolve. The mask openings are an inverse copy of the resist pattern which is to remain on the wafer.


* '''Thickness of resist''': In general, it is recommended to work at or below an aspect ratio of ~1, i.e. where the width of the pattern is larger than the thickness of the resist. Furthermore, when you decide the resist thickness, consider which transfer you need:
'''Pre-cleanroom work:'''
** For <u>[[Specific_Process_Knowledge/Lithography/LiftOff|lift-off]]</u> processes, we recommend resist thickness at least 5 times larger than the thickness of the metal to be lifted.
# Complete the [https://labadviser.nanolab.dtu.dk//index.php?title=Specific_Process_Knowledge/Lithography#Lithography_Tool_Package_Training Lithography TPT]
** For dry etch or wet etch processes, investigate the resist etch rate of your process as this might limit the minimum thickness of your resist.
# Prepare a process flow: The process flow describes all steps in your UV lithography process. You can find docx-templates <u>[[Specific_Process_Knowledge/Lithography/Resist/UVresist#UV_resist_comparison_table|in this table]]</u>
# Evaluate your process in cooperation with the fabrication support group
# Design device: Design your device and layout. A detailed instruction on how to design a layout (or mask) can be found <u>[[Specific_Process_Knowledge/Pattern_Design|here]]</u>
# Mask: If you wish to use a mask aligner, order a photomask for your UV process. Instructions on how to order a photomask can be found <u>[[Specific_Process_Knowledge/Pattern_Design#Mask_Ordering_and_Fabrication|here]]</u>


* '''Spin Coater''': Do you wish to use a manual spin coater or an automatic spin coater? See a list of spin coaters <u>[[Specific_Process_Knowledge/Lithography/Coaters|here]]</u>.


*'''Exposure''': Choose which aligner you wish to use, and consider the exposure dose.
'''Cleanroom work:'''
** You can find a list of mask aligners and maskless aligners <u>[[Specific_Process_Knowledge/Lithography/UVExposure|here]]</u>.
# Substrate pretreatment: In many processes it is recommended to <u>[[Specific_Process_Knowledge/Lithography/Pretreatment|pre-treat or prime]]</u> your wafer before coating. In some <u>[[Specific_Process_Knowledge/Lithography/Coaters|spin coaters]]</u>, these pre-treatment processes are included in the spin coating of resist
** You can find information on dose <u>[[Specific_Process_Knowledge/Lithography/UVExposure_Dose|here]]</u>.
# Resist Type: Choose the type of resist you wish to use: a list of UV lithography resist types available at DTU Nanolab can be found <u>[[Specific_Process_Knowledge/Lithography/Resist#UV_Resist|on this page]]</u>
#*Positive tone resist: Resist exposed to UV light will be dissolved in the developer. For mask aligners, the mask openings are an exact copy of the resist pattern which is to remain on the wafer
#*Negative tone resist: Resist exposed to UV light will become polymerized and difficult to dissolve. For mask aligners, the mask openings are an ''inverse'' copy of the resist pattern which is to remain on the wafer
# Thickness of resist: In general, it is recommended to work at, or below, an aspect ratio of ~1, i.e. where the feature sizes of the pattern, is larger than the thickness of the resist. Furthermore, when you decide on the resist thickness, consider which transfer method you need:
#*For <u>[[Specific_Process_Knowledge/Lithography/LiftOff|lift-off]]</u> processes, we recommend resist thickness at least 5 times larger than the thickness of the metal to be lifted
#*For dry etch or wet etch processes, investigate the resist etch rate of your process, as this might limit the ''minimum'' thickness of your resist
# Spin Coater: Do you need to use a manual spin coater or an automatic spin coater? See a list of spin coaters <u>[[Specific_Process_Knowledge/Lithography/Coaters|here]]</u>
# Exposure: Choose which aligner you wish to use, and consider the exposure dose
#*You can find a list of mask aligners and maskless aligners <u>[[Specific_Process_Knowledge/Lithography/UVExposure|here]]</u>
#*You can find information on dose <u>[[Specific_Process_Knowledge/Lithography/Resist#UV_Resist|here]]</u>
# Development: Choose which equipment you wish to use to develop your photoresist from <u>[[Specific_Process_Knowledge/Lithography/Development|this list]]</u>. Remember the development process influences the <u>[[Specific_Process_Knowledge/Lithography/Resist#UV_Resist|exposure dose]]</u>
# Specify whether you wish to strip or lift-off your resist: <u>[[Specific_Process_Knowledge/Lithography/Strip|strip]]</u> and <u>[[Specific_Process_Knowledge/Lithography/LiftOff|lift-off]]</u>


* '''Mask''': If you wish to use a mask aligner, order a photomask for your UV process. Instructions on how to order a photomask can be found <u>[[Specific_Process_Knowledge/Pattern_Design#Mask_Ordering_and_Fabrication|here]]</u>.


* '''Development''': Choose which equipment you wish to use to develop your photoresist from <u>[[Specific_Process_Knowledge/Lithography/Development|this list]]</u>. Remember the development process influences the <u>[[Specific_Process_Knowledge/Lithography/UVExposure_Dose|exposure dose]]</u>.
==Mask Aligner versus Maskless Aligner==


* '''Specify whether you wish to strip or lift-off your resist''': <u>[[Specific_Process_Knowledge/Lithography/Strip|strip]]</u> and <u>[[Specific_Process_Knowledge/Lithography/LiftOff|lift-off]]</u>.
[[Specific_Process_Knowledge/Lithography/Aligners/MAvsMLA|Mask Aligner vs Maskless Aligner]]


<br clear=all />
<br clear=all />


= Resist Overview =
<!---
 
=Equipment and Process Pages=
{|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" width="90%"
{{:Specific Process Knowledge/Lithography/UVlithographyProcessPages}}
|-
 
|-
|-style="background:silver; color:black"
|'''Resist'''
|width=100|'''Polarity'''
|'''Spectral sensitivity'''
|'''Manufacturer'''
|width=200|'''Comments'''
|width=100|'''Technical reports'''
|'''[[Specific_Process_Knowledge/Lithography/Coaters|Spin Coating]]'''
|'''[[Specific_Process_Knowledge/Lithography/UVExposure|Exposure]]'''
|'''[[Specific_Process_Knowledge/Lithography/Development|Developer]]'''
|'''Rinse'''
|width=100|'''Remover'''
|'''Process flows (in docx-format)'''
 
|-
 
|-
|-style="background:WhiteSmoke; color:black"
|'''[[Specific_Process_Knowledge/Lithography/5214E|AZ 5214E]]'''
|Positive but the image can be reversed
|310 - 420 nm
|[https://www.merckgroup.com/en/brands/pm/az-products.html Merck KGaA]
 
Supplied by [https://www.microchemicals.com/ MicroChemicals GmbH]
|Can be used for both positive and image reversed (negative) processes with resist thickness between 1 and 4 µm.
|[[media:AZ5214E.pdf‎|AZ5214E.pdf‎]]
 
[https://www.microchemicals.com/micro/tds_az_5214e_photoresist.pdf Photoresist AZ® 5214 E (TDS)]
|Automatic spin coater ([[Specific_Process_Knowledge/Lithography/Coaters#Spin_Coater:_Gamma_UV|Gamma UV]] or [[Specific_Process_Knowledge/Lithography/Coaters#Spin_Coater:_Gamma_E-beam_and_UV|Gamma e-beam & UV]])
 
Manual spin coater ([[Specific_Process_Knowledge/Lithography/Coaters#Manual_Spin_Coaters|LabSpin]] or [[Specific_Process_Knowledge/Lithography/Coaters#Spin_Coater:_RCD8|RCD8]])
|Mask aligner ([[Specific_Process_Knowledge/Lithography/UVExposure#KS_Aligner|KS]] or [[Specific_Process_Knowledge/Lithography/UVExposure#Aligner:_MA6_-_2|MA6 - 2]])
 
Maskless aligner ([[Specific_Process_Knowledge/Lithography/UVExposure#Aligner:_Maskless_01|01]], [[Specific_Process_Knowledge/Lithography/UVExposure#Aligner:_Maskless_02|02]] or [[Specific_Process_Knowledge/Lithography/UVExposure#Aligner:_Maskless_03|03]])
|AZ 351B developer
or
 
[[Specific_Process_Knowledge/Lithography/Development#Developer_TMAH_UV-lithography|AZ 726 MIF developer]]
|DI water
|Acetone
|
Mask aligner:
[[media:‎Process_Flow_AZ5214E_pos_vers2.docx‎ |Process_Flow_AZ5214_pos.docx‎]]
[[media:Process_Flow_AZ5214E_rev_vers2.docx‎ |Process_Flow_AZ5214_rev.docx‎]]
 
Maskless aligner:
[[media:‎Process_Flow_AZ5214E_MLA_pos.docx‎ |Process_Flow_AZ5214_MLA_pos.docx‎]]
[[media:Process_Flow_AZ5214E_MLA_rev.docx‎ |Process_Flow_AZ5214_MLA_rev.docx‎]]
 
|-
|-style="background:LightGrey; color:black"
|'''[[Specific_Process_Knowledge/Lithography/4562|AZ 4562]]'''
|Positive
|310 - 440 nm
|[https://www.merckgroup.com/en/brands/pm/az-products.html Merck KGaA]
 
Supplied by [https://www.microchemicals.com/ MicroChemicals GmbH]
|For process with resist thickness between 6 and 25 µm.
|[[media:AZ4500.pdf‎|AZ4500.pdf‎]]
 
[https://www.microchemicals.com/micro/tds_az_4500_series.pdf Photoresist AZ® 4562 (TDS)]
|Automatic spin coater ([[Specific_Process_Knowledge/Lithography/Coaters#Spin_Coater:_Gamma_E-beam_and_UV|Gamma e-beam & UV]])
 
Manual spin coater ([[Specific_Process_Knowledge/Lithography/Coaters#Manual_Spin_Coaters|LabSpin]] or [[Specific_Process_Knowledge/Lithography/Coaters#Spin_Coater:_RCD8|RCD8]])
|Mask aligner ([[Specific_Process_Knowledge/Lithography/UVExposure#KS_Aligner|KS]] or [[Specific_Process_Knowledge/Lithography/UVExposure#Aligner:_MA6_-_2|MA6 - 2]])
 
Maskless aligner ([[Specific_Process_Knowledge/Lithography/UVExposure#Aligner:_Maskless_01|01]] or [[Specific_Process_Knowledge/Lithography/UVExposure#Aligner:_Maskless_03|03]])
|AZ 351B developer
or
 
[[Specific_Process_Knowledge/Lithography/Development#Developer_TMAH_UV-lithography|AZ 726 MIF developer]]
|DI water
|Acetone
|
Mask aligner:
[[media:Process_Flow_thick_AZ4562_vers2.docx‎|Process_Flow_thick_AZ4562.docx‎]]
 
Maskless aligner:
[[media:Process_Flow_thick_AZ4562_MLA.docx‎|Process_Flow_thick_AZ4562_MLA.docx‎]]
 
|-
|-style="background:WhiteSmoke; color:black"
|'''[[Specific_Process_Knowledge/Lithography/MiR|AZ MiR 701]]'''
|Positive
|310 - 445 nm
|[https://www.merckgroup.com/en/brands/pm/az-products.html Merck KGaA]
 
Supplied by [https://www.microchemicals.com/ MicroChemicals GmbH]
|High selectivity for dry etch.
 
Resist thickness 1.5 - 4 µm.
|[[media:AZ_MiR_701.pdf‎|AZ_MiR_701.pdf‎]]
 
[https://www.microchemicals.com/micro/tds_az_mir701_photoresist.pdf Photoresist AZ® MIR 701 (TDS)]
|Automatic spin coater ([[Specific_Process_Knowledge/Lithography/Coaters#Spin_Coater:_Gamma_UV|Gamma UV]] or [[Specific_Process_Knowledge/Lithography/Coaters#Spin_Coater:_Gamma_E-beam_and_UV|Gamma e-beam & UV]])
 
Manual spin coater ([[Specific_Process_Knowledge/Lithography/Coaters#Manual_Spin_Coaters|LabSpin]] or [[Specific_Process_Knowledge/Lithography/Coaters#Spin_Coater:_RCD8|RCD8]])
|
Mask aligner ([[Specific_Process_Knowledge/Lithography/UVExposure#KS_Aligner|KS]] or [[Specific_Process_Knowledge/Lithography/UVExposure#Aligner:_MA6_-_2|MA6 - 2]])
 
Maskless aligner ([[Specific_Process_Knowledge/Lithography/UVExposure#Aligner:_Maskless_01|01]], [[Specific_Process_Knowledge/Lithography/UVExposure#Aligner:_Maskless_02|02]] or [[Specific_Process_Knowledge/Lithography/UVExposure#Aligner:_Maskless_03|03]])
|[[Specific_Process_Knowledge/Lithography/Development#Developer_TMAH_UV-lithography|AZ 726 MIF developer]]
|DI water
|Remover 1165
|
Mask aligner:
[[media:Process_Flow_AZ_MiR701.docx‎|Process_Flow_AZ_MiR701.docx‎]]
 
Maskless aligner:
[[media:Process_Flow_AZ_MiR701_MLA.docx‎|Process_Flow_AZ_MiR701_MLA.docx‎]]
 
|-
|-style="background:LightGrey; color:black"
|'''[[Specific_Process_Knowledge/Lithography/nLOF|AZ nLOF 2020]]'''
|Negative
|310 - 380 nm
|[https://www.merckgroup.com/en/brands/pm/az-products.html Merck KGaA]
 
Supplied by [https://www.microchemicals.com/ MicroChemicals GmbH]
|Negative sidewalls for lift-off.
 
Resist thickness 1.5 - 4 µm.
|[[media:AZ_nLOF_2020.pdf‎|AZ_nLOF_2020.pdf‎]]
 
[https://www.microchemicals.com/micro/tds_az_nlof2000_series.pdf Photoresist AZ®nLOF 2020 (TDS)]
|Automatic spin coater ([[Specific_Process_Knowledge/Lithography/Coaters#Spin_Coater:_Gamma_UV|Gamma UV]])
 
Manual spin coater ([[Specific_Process_Knowledge/Lithography/Coaters#Manual_Spin_Coaters|LabSpin]] or [[Specific_Process_Knowledge/Lithography/Coaters#Spin_Coater:_RCD8|RCD8]])
|
Mask aligner ([[Specific_Process_Knowledge/Lithography/UVExposure#KS_Aligner|KS]] or [[Specific_Process_Knowledge/Lithography/UVExposure#Aligner:_MA6_-_2|MA6 - 2]])
 
Maskless aligner ([[Specific_Process_Knowledge/Lithography/UVExposure#Aligner:_Maskless_01|01]] or [[Specific_Process_Knowledge/Lithography/UVExposure#Aligner:_Maskless_02|02]])
|[[Specific_Process_Knowledge/Lithography/Development#Developer_TMAH_UV-lithography|AZ 726 MIF developer]]
|DI water
|Remover 1165
|
Mask aligner:
[[media:Process_Flow_AZ_nLOF_2020.docx‎|Process_Flow_AZ_nLOF_2020.docx‎]]
 
Maskless aligner:
[[media:Process_Flow_AZ_nLOF_2020_MLA.docx‎|Process_Flow_AZ_nLOF_2020_MLA.docx‎]]
 
|-
|-style="background:WhiteSmoke; color:black"
|'''[[Specific Process Knowledge/Lithography/SU-8|SU-8]]'''
|Negative
|350 - 400 nm
|[https://kayakuam.com/products/su-8-2000/ Kayaku Advanced Materials, Inc.]
 
Supplied by [http://www.microresist.com/products/ micro resist technology GmbH]
|High aspect ratio.
 
Resist thickness 1 µm to several 100 µm.
|[[media:SU-8_DataSheet_2005.pdf‎|SU-8_DataSheet_2005.pdf‎]], [[media:SU-8_DataSheet_2075.pdf‎|SU-8_DataSheet_2075.pdf‎]]
|Manual spin coater ([[Specific_Process_Knowledge/Lithography/Coaters#Manual_Spin_Coaters|LabSpin]] or [[Specific_Process_Knowledge/Lithography/Coaters#Spin_Coater:_RCD8|RCD8]])
|
Mask aligner ([[Specific_Process_Knowledge/Lithography/UVExposure#KS_Aligner|KS]] or [[Specific_Process_Knowledge/Lithography/UVExposure#Aligner:_MA6_-_2|MA6 - 2]])
 
Maskless aligner ([[Specific_Process_Knowledge/Lithography/UVExposure#Aligner:_Maskless_01|01]] or [[Specific_Process_Knowledge/Lithography/UVExposure#Aligner:_Maskless_02|02]])
|[[Specific_Process_Knowledge/Lithography/Development#SU8-Developer|mr-Dev 600 developer (PGMEA)]]
|IPA
|Plasma ashing can remove crosslinked SU-8
|[[media:Process_Flow_SU8_70um.docx‎|Process_Flow_SU8_70um.docx‎]]
 
Most of the process knowledge on SU-8 is based in research groups
 
|}
 
 
===Other process flows===
*[[media:Process_Flow_ChipOnCarrier.docx‎|Process_Flow_ChipOnCarrier.docx‎]]: A procedure for UV lithography on a chip using automatic coater and developer.
 
<br clear="all" />
 
=Process information=


===[[Specific Process Knowledge/Lithography/Resist#UV_Resist|UV Resist]]===
===[[Specific Process Knowledge/Lithography/Pretreatment|Pretreatment]]===
===[[Specific Process Knowledge/Lithography/Pretreatment|Pretreatment]]===
===[[Specific Process Knowledge/Lithography/Coaters|Coaters]]===
===[[Specific Process Knowledge/Lithography/Coaters|Coating]]===
===[[Specific Process Knowledge/Lithography/UVExposure|UV Exposure]]===
====[[Specific_Process_Knowledge/Lithography/UVExposure_Dose|Information on UV Exposure Dose]]====
===[[Specific Process Knowledge/Lithography/Baking|Baking]]===
===[[Specific Process Knowledge/Lithography/Baking|Baking]]===
===[[Specific Process Knowledge/Lithography/UVExposure|UV Exposure Tools]]===
===[[Specific Process Knowledge/Lithography/Development|Development]]===
===[[Specific Process Knowledge/Lithography/Development|Development]]===
===[[Specific Process Knowledge/Lithography/Descum|Descum]]===
===[[Specific Process Knowledge/Lithography/Descum|Descum]]===
===[[Specific Process Knowledge/Lithography/LiftOff|Lift-off]]===
===[[Specific Process Knowledge/Lithography/Strip|Stripping Resist]]===
===[[Specific Process Knowledge/Lithography/Strip|Stripping Resist]]===
===[[Specific Process Knowledge/Lithography/LiftOff|Lift-off]]===
--->


===Information from our suppliers===
=Process information from our suppliers=
MicroChemicals GmbH has a [https://www.microchemicals.com/downloads/application_notes.html very large online library] of information about UV lithography.


[https://www.microchemicals.com/downloads/application_notes.html Application notes] from MicroChemicals GmbH, e.g. [https://www.microchemicals.com/technical_information/lithography_trouble_shooting.pdf Lithography Trouble-Shooter]
Of particular interest is the [https://www.microchemicals.com/dokumente/application_notes/lithography_trouble_shooting.pdf lithography trouble-shooter]

Latest revision as of 09:12, 4 June 2026

The content on this page, including all images and pictures, was created by DTU Nanolab staff, unless otherwise stated.

Feedback to this page: click here

UV lithography

UV Lithography uses ultraviolet light to transfer a pattern from a photo-mask, or a digital design file, to a substrate coated with photoresist.

The process has 3 main steps:

  1. Coating the substrate with a photosensitive film
  2. Transferring a pattern into the resist by exposing it with UV light through either a physical shadow mask or a digital version of a shadow mask
  3. Developing the exposed resist to reveal the transferred pattern

DTU Nanolab offers a number of automatic and manual coaters, mask or maskless exposure tools, as well as automatic or semi-automatic developers.

Getting started with UV lithography

New users are always recommended to have their process evaluated by the fabrication support group - before you start planning your UV process, and request training on UV lithography equipment, please go through the following pre-cleanroom and cleanroom steps and include all the information in your request.

Please remember that the Lithography TPT is mandatory before you can receive training on any lithography equipment.
If you are completely new to photolithography, you can visit this wikipedia webpage about photolithography before you start.


Pre-cleanroom work:

  1. Complete the Lithography TPT
  2. Prepare a process flow: The process flow describes all steps in your UV lithography process. You can find docx-templates in this table
  3. Evaluate your process in cooperation with the fabrication support group
  4. Design device: Design your device and layout. A detailed instruction on how to design a layout (or mask) can be found here
  5. Mask: If you wish to use a mask aligner, order a photomask for your UV process. Instructions on how to order a photomask can be found here


Cleanroom work:

  1. Substrate pretreatment: In many processes it is recommended to pre-treat or prime your wafer before coating. In some spin coaters, these pre-treatment processes are included in the spin coating of resist
  2. Resist Type: Choose the type of resist you wish to use: a list of UV lithography resist types available at DTU Nanolab can be found on this page
    • Positive tone resist: Resist exposed to UV light will be dissolved in the developer. For mask aligners, the mask openings are an exact copy of the resist pattern which is to remain on the wafer
    • Negative tone resist: Resist exposed to UV light will become polymerized and difficult to dissolve. For mask aligners, the mask openings are an inverse copy of the resist pattern which is to remain on the wafer
  3. Thickness of resist: In general, it is recommended to work at, or below, an aspect ratio of ~1, i.e. where the feature sizes of the pattern, is larger than the thickness of the resist. Furthermore, when you decide on the resist thickness, consider which transfer method you need:
    • For lift-off processes, we recommend resist thickness at least 5 times larger than the thickness of the metal to be lifted
    • For dry etch or wet etch processes, investigate the resist etch rate of your process, as this might limit the minimum thickness of your resist
  4. Spin Coater: Do you need to use a manual spin coater or an automatic spin coater? See a list of spin coaters here
  5. Exposure: Choose which aligner you wish to use, and consider the exposure dose
    • You can find a list of mask aligners and maskless aligners here
    • You can find information on dose here
  6. Development: Choose which equipment you wish to use to develop your photoresist from this list. Remember the development process influences the exposure dose
  7. Specify whether you wish to strip or lift-off your resist: strip and lift-off


Mask Aligner versus Maskless Aligner

Mask Aligner vs Maskless Aligner



Process information from our suppliers

MicroChemicals GmbH has a very large online library of information about UV lithography.

Of particular interest is the lithography trouble-shooter