AZ MiR 701 is a positive UV photoresist.
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/MiR click here]'''
 
[[Category: Lithography|Resist]]
[[Category: Resist|AZ MiR 701]]
 
__TOC__
 
==Resist description==
AZ MiR 701 is a positive UV photoresist. It is considered to have high selectivity for dry etching.


==Spin coating==
==Spin coating==
[[Image:MiRspincurves.JPG|640px|thumb|Spin curves for AZ MiR 701 (29 cps) using a 30 s spin-off, and a 60 s @ 90°C proximity softbake]]


[[Image:MiRspincurves.JPG|500x500px|thumb|Spin curves for AZ MiR 701 (29cps) using a 30s spin-off, and a 60s@90°C softbake (proximity bake for Gamma)]]
'''Typical spin parameters:'''
 
*Spin off: 30-60 s
*Soft bake: 60 s @ 90°C in proximity
<br clear="all" />
<br clear="all" />


==Exposure==
==Exposure==
'''Dehydration of resist film:'''<br>
During exposure in the maskless aligners, MiR can be sensitive to dehydration by the air flow applied by the pneumatic auto-focus mechanism. This may lead to insufficient development, especially for small substrates. This problem can be alleviated by switching to the overview camera for a period of 1 minute before starting the exposure, or simply by parking the writehead away from the exposure location for 1 minute before starting the exposure.


During exposure using the maskless aligners, MiR can be sensitive to dehydration by the air flow applied by the pneumatic auto-focus mechanism. This may lead to insufficient development, especially for small substrates. This problem can be alleviated by switching to the overview camera for a period of 1-2 minutes before starting the exposure. The effect can also be reduced by increasing the soft bake.
The effect can also be reduced by increasing the soft bake.


==Post-exposure bake==
==Post-exposure bake==
'''Typical PEB parameters:'''
*PEB temperature: 110°C
*PEB time: 60 s


During exposure, interaction between the incoming light and the light reflected by the substrate can cause a standing wave to form in the resist (especially true for single line/wavelength exposure). This leads to a wavy sidewall after development. The standing wave pattern can be removed by introducing a post-exposure bake before development, which allows the activated PAC to diffuse into un-activated regions, thus smoothing the sidewall. The recommended PEB for MiR is 60s at 110°C (1-2µm film). Thicker coatings may require longer bake, and substrate thickness and material, e.g glass, may also affect the required baking time.


As the post-exposure bake is at an elevated temperature compared to the soft bake, it will cause the resist film to become 5-10% thinner (probably due to continued evaporation of solvent). A 1.5µm thick MiR resist film will be approximately 1.4µm after PEB.
During exposure, interaction between the incoming light and the light reflected by the substrate can cause a standing wave to form in the resist (especially true for single line/wavelength exposure). This leads to a wavy sidewall after development. The standing wave pattern can be reduced by introducing a post-exposure bake before development, which allows the activated PAC to diffuse into un-activated regions, thus smoothing the sidewall. The recommended PEB for MiR is 60 s at 110°C (for a 1 - 2 µm film). Thicker coatings may require longer bake, and substrate thickness and material may also affect the required baking time.
 
Since the post-exposure bake is at an elevated temperature compared to the soft bake, it will cause the resist film to become 5-10% thinner (probably due to continued evaporation of solvent). A 1.5 µm thick MiR resist film will be approximately 1.4 µm after PEB.
 
<gallery style="text-align: center;" widths=450 heights=350>
MIR_noPEB.jpg|1.5 µm AZ MIR 701 without PEB
MIR_withPEB.jpg|1.5 µm AZ MIR 701 with PEB
</gallery>


==Development==
==Development==
 
'''Development speed:'''
A 1.5-2µm MiR resist film is fully developed in 60s using TMAH (AZ 726). Depending on the exposure dose, thicker coatings may develop in 1 min, but it is probably better to aim for a similar development speed (2µm/min).
*Puddle development in 2.38% TMAH (AZ 726 MIF): ~2 µm/min