Specific Process Knowledge/Etch/Etching of Chromium: Difference between revisions
Appearance
| (15 intermediate revisions by 4 users not shown) | |||
| Line 1: | Line 1: | ||
'''Feedback to this page''': '''[mailto:labadviser@ | '''Unless anything else is stated, everything on this page, text and pictures are made by DTU Nanolab.''' | ||
'''All links to Kemibrug (SDS) and Labmanager Including APV and QC requires login.''' | |||
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/Etching_of_Chromium click here]''' | |||
<!--Page reviewed by jmli 1/8-2016 --> | |||
<!--Page reviewed by jmli 9/8-2022 --> | |||
==Etching of Chromium== | ==Etching of Chromium== | ||
| Line 5: | Line 12: | ||
Etching of chromium can be done either by wet etch, dry etch or by sputtering with ions. | Etching of chromium can be done either by wet etch, dry etch or by sputtering with ions. | ||
*[[Specific Process Knowledge/Etch/Wet Chromium Etch|Etching of Cr by wet etch]] | *[[Specific Process Knowledge/Etch/Wet Chromium Etch|Etching of Cr by wet etch]] | ||
*[[Specific Process Knowledge/Etch/ICP Metal Etcher/Chromium|Etching of Cr by | *[[Specific Process Knowledge/Etch/ICP Metal Etcher/Chromium|Etching of Cr by ICP metal]] | ||
*[[Specific_Process_Knowledge/Etch/IBE⁄IBSD Ionfab 300|Sputtering of Cr]] | *[[Specific_Process_Knowledge/Etch/IBE⁄IBSD Ionfab 300|Sputtering of Cr]] | ||
<br clear="all" /> | <br clear="all" /> | ||
==Comparison of Chromium Etch | ==Comparison of Chromium Etch Methods== | ||
{|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" | {|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" | ||
| Line 17: | Line 24: | ||
|-style="background:silver; color:black" | |-style="background:silver; color:black" | ||
! | ! | ||
![[Specific Process Knowledge/Etch/Wet Chromium Etch|Cr wet etch | ![[Specific Process Knowledge/Etch/Wet Chromium Etch|Cr wet etch]] | ||
![[Specific_Process_Knowledge/Etch/ICP_Metal_Etcher|ICP metal]] | ![[Specific_Process_Knowledge/Etch/ICP_Metal_Etcher|ICP metal]] | ||
![[Specific_Process_Knowledge/Etch/IBE⁄IBSD Ionfab 300|IBE (Ionfab300+)]] | ![[Specific_Process_Knowledge/Etch/IBE⁄IBSD Ionfab 300|IBE (Ionfab300+)]] | ||
![[Specific_Process_Knowledge/Etch/DRIE-Pegasus/Pegasus-2|DRIE-Pegasus 2]] | |||
|- | |- | ||
|- | |- | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
! | !General description | ||
|Wet etch of Cr premixed (Chrome etch 18) | |Wet etch of Cr premixed (Chrome etch 18) | ||
|Dry plasma etch of Cr | |Dry plasma etch of Cr | ||
|Sputtering of Cr - pure physical etch | |Sputtering of Cr - pure physical etch | ||
|Primarily shallow dry etching of silicon but also thin layers of SiO2, TaO2 and Cr | |||
|- | |- | ||
| Line 36: | Line 43: | ||
!Etch rate range | !Etch rate range | ||
| | | | ||
*~ | *~150nm/min at room temperature | ||
| | | | ||
*~14 nm/min (depending on features size and etch load) | *~14 nm/min (depending on features size and etch load) | ||
| | | | ||
*~30nm/min (not tested yet) | *~30nm/min (not tested yet) | ||
| | |||
* very slow | |||
|- | |- | ||
| Line 48: | Line 55: | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
!Etch profile | !Etch profile | ||
| | | | ||
*Isotropic | *Isotropic | ||
| Line 56: | Line 61: | ||
| | | | ||
*Anisotropic (angles sidewalls, typical around 70 dg) | *Anisotropic (angles sidewalls, typical around 70 dg) | ||
| | |||
*Anisotropic (vertical sidewalls) | |||
|- | |- | ||
|- | |- | ||
| Line 65: | Line 71: | ||
*Any size and number that can go inside the beaker in use | *Any size and number that can go inside the beaker in use | ||
| | | | ||
* | * 150 mm wafers | ||
* Smaller wafers or pieces on a 150 mm carrier wafer | |||
* | |||
| | | | ||
Smaller pieces glued to carrier wafer | Smaller pieces glued to carrier wafer | ||
* | * 50mm wafer | ||
* | * 100mm wafer | ||
* | * 150mm wafer | ||
* | * 200mm wafer | ||
| | |||
* 150mm wafer | |||
* Smaller wafers or pieces on 150mm carrier | |||
|- | |- | ||
|- | |- | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
! | !Allowed materials | ||
| | | | ||
No restrictions cross contamination wise as long as you use the right beaker and make sure that they are safe to enter in the chemicals | No restrictions cross contamination wise as long as you use the right beaker and make sure that they are safe to enter in the chemicals | ||
| Line 108: | Line 112: | ||
*Polymers | *Polymers | ||
*Capton tape | *Capton tape | ||
| | |||
* Silicon | |||
* Silicon oxides | |||
* Silicon nitrides | |||
* Thin layers of Cr, TaO2 | |||
|- | |- | ||
|} | |} | ||
Latest revision as of 09:33, 8 April 2026
Unless anything else is stated, everything on this page, text and pictures are made by DTU Nanolab.
All links to Kemibrug (SDS) and Labmanager Including APV and QC requires login.
Feedback to this page: click here
Etching of Chromium
Etching of chromium can be done either by wet etch, dry etch or by sputtering with ions.
Comparison of Chromium Etch Methods
| Cr wet etch | ICP metal | IBE (Ionfab300+) | DRIE-Pegasus 2 | |
|---|---|---|---|---|
| General description | Wet etch of Cr premixed (Chrome etch 18) | Dry plasma etch of Cr | Sputtering of Cr - pure physical etch | Primarily shallow dry etching of silicon but also thin layers of SiO2, TaO2 and Cr |
| Etch rate range |
|
|
|
|
| Etch profile |
|
|
|
|
| Substrate size |
|
|
Smaller pieces glued to carrier wafer
|
|
| Allowed materials |
No restrictions cross contamination wise as long as you use the right beaker and make sure that they are safe to enter in the chemicals |
|
|
|