'''Unless anything else is stated, everything on this page, text and pictures are made by DTU Nanolab.'''
 
'''All links to Kemibrug (SDS) and Labmanager Including APV and QC requires login.'''
 
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/Etching_of_Chromium click here]'''
<!--Page reviewed by jmli 1/8-2016  -->
<!--Page reviewed by jmli 1/8-2016  -->
<!--Page reviewed by jmli 9/8-2022  -->
==Etching of Chromium==
==Etching of Chromium==


Line 20: Line 27:
![[Specific_Process_Knowledge/Etch/ICP_Metal_Etcher|ICP metal]]
![[Specific_Process_Knowledge/Etch/ICP_Metal_Etcher|ICP metal]]
![[Specific_Process_Knowledge/Etch/IBE&frasl;IBSD Ionfab 300|IBE (Ionfab300+)]]
![[Specific_Process_Knowledge/Etch/IBE&frasl;IBSD Ionfab 300|IBE (Ionfab300+)]]
![[Specific_Process_Knowledge/Etch/DRIE-Pegasus/Pegasus-2|DRIE-Pegasus 2]]
|-
|-


|-
|-
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
!Generel description
!General description
|Wet etch of Cr premixed (Chrome etch 18)
|Wet etch of Cr premixed (Chrome etch 18)
|Dry plasma etch of Cr
|Dry plasma etch of Cr
|Sputtering of Cr - pure physical etch
|Sputtering of Cr - pure physical etch
|Primarily shallow dry etching of silicon but also thin layers of SiO2, TaO2 and Cr
|-
|-


Line 39: Line 48:
|  
|  
*~30nm/min (not tested yet)  
*~30nm/min (not tested yet)  
|
* very slow
|-
|-


Line 50: Line 61:
|
|
*Anisotropic (angles sidewalls, typical around 70 dg)
*Anisotropic (angles sidewalls, typical around 70 dg)
|
*Anisotropic (vertical sidewalls)
|-
|-


|-
|-
Line 59: Line 71:
*Any size and number that can go inside the beaker in use
*Any size and number that can go inside the beaker in use
|
|
*smaller pieces on a carrier wafer
* 150 mm wafers
*<nowiki>#</nowiki>1 100mm wafers (when set up to 100mm wafers)
* Smaller wafers or pieces on a 150 mm carrier wafer
*<nowiki>#</nowiki>1 150mm wafers (when set up to 150mm wafers)
|
|
Smaller pieces glued to carrier wafer
Smaller pieces glued to carrier wafer
*<nowiki>#</nowiki>1 50mm wafer
* 50mm wafer
*<nowiki>#</nowiki>1 100mm wafer
* 100mm wafer
*<nowiki>#</nowiki>1 150mm wafer
* 150mm wafer
*<nowiki>#</nowiki>1 200mm wafer
* 200mm wafer
|
* 150mm wafer
* Smaller wafers or pieces on 150mm carrier
|-
|-


|-
|-
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
!'''Allowed materials'''
!Allowed materials
|
|
No restrictions cross contamination wise as long as you use the right beaker and make sure that they are safe to enter in the chemicals
No restrictions cross contamination wise as long as you use the right beaker and make sure that they are safe to enter in the chemicals
Line 98: Line 112:
*Polymers
*Polymers
*Capton tape
*Capton tape
|
* Silicon
* Silicon oxides
* Silicon nitrides
* Thin layers of Cr, TaO2
|-
|-


|}
|}

Latest revision as of 09:33, 8 April 2026

Unless anything else is stated, everything on this page, text and pictures are made by DTU Nanolab.

All links to Kemibrug (SDS) and Labmanager Including APV and QC requires login.

Feedback to this page: click here


Etching of Chromium

Etching of chromium can be done either by wet etch, dry etch or by sputtering with ions.


Comparison of Chromium Etch Methods

Cr wet etch ICP metal IBE (Ionfab300+) DRIE-Pegasus 2
General description Wet etch of Cr premixed (Chrome etch 18) Dry plasma etch of Cr Sputtering of Cr - pure physical etch Primarily shallow dry etching of silicon but also thin layers of SiO2, TaO2 and Cr
Etch rate range
  • ~150nm/min at room temperature
  • ~14 nm/min (depending on features size and etch load)
  • ~30nm/min (not tested yet)
  • very slow
Etch profile
  • Isotropic
  • Anisotropic (vertical sidewalls)
  • Anisotropic (angles sidewalls, typical around 70 dg)
  • Anisotropic (vertical sidewalls)
Substrate size
  • Any size and number that can go inside the beaker in use
  • 150 mm wafers
  • Smaller wafers or pieces on a 150 mm carrier wafer

Smaller pieces glued to carrier wafer

  • 50mm wafer
  • 100mm wafer
  • 150mm wafer
  • 200mm wafer
  • 150mm wafer
  • Smaller wafers or pieces on 150mm carrier
Allowed materials

No restrictions cross contamination wise as long as you use the right beaker and make sure that they are safe to enter in the chemicals

  • Silicon
  • Quartz/fused silica
  • Photoresist/e-beam resist
  • PolySilicon,
  • Silicon oxide
  • Silicon (oxy)nitride
  • Aluminium
  • Titanium
  • Chromium
  • Silicon
  • Silicon oxides
  • Silicon nitrides
  • Metals from the +list
  • Metals from the -list
  • Alloys from the above list
  • Stainless steel
  • Glass
  • III-V materials
  • Resists
  • Polymers
  • Capton tape
  • Silicon
  • Silicon oxides
  • Silicon nitrides
  • Thin layers of Cr, TaO2