==SiO2 Etch using aSi as masking material==
===Uniformity results with SiO2_res_10===
[[File:SiO2 etch uniformity DOE3_10.JPG|400px|thumb|left|Etched for 3min56s, average etch rate: 250 nm/min +- 2.9% ]]
<br clear="all"/>
 
===Results with SiO2_res_10 and with with the electro magnets on===
The SiO2:res_10 recipe was tested with the electromagnets on but it seems to no no good for the results.[[File:Contour Plot Y31 EM_02_30 white to blue.jpg|400px|thumb|left|Etched with EM:02/30 for 2min, average etch rate: 275 nm/min +- 4.5%. The electro magnets changed the uniformity pattern and made it a bit worse ]]
<br clear="all"/>
 
<gallery caption="Recipe name: SiO2_res_10, Recipe no. 10+EM coils: C06445_02 coil_2500W, platen:300W, EM:02/30A, He/C4F8= 17.5, C4F8/H2=1, Pressure:8.8mTorr, C4F8:25.6sccm, He:448.7sccm, H2:25.6sccm, 3:56 min " perrow="5">


{{CC-bghe2}} <br>
File:C09936_05.jpg
I am now starting up development of SiO2 etch using aSi as masking material. <br>
File:C09936_04.jpg
The samples I use are:  
File:C09936_03.jpg
*6" Si afters with oxide (2µm),
File:C09936_02.jpg
*aSi (~300nm),
File:C09936_01.jpg
*Neg. DUV reist (~60nm barc, ~350 nm resist)
</gallery>
*Reticle: Danchip/Triple-D
*Dose 230 J/m2
First I need to make sure that the resist work for pattering the aSi layer is good. If the resist is not good the final etch will also not be good.


===DUV optimization===
Using the electromagnetic coil on the recipe SiO2_res_10 gave higher etch rate on this chip, which is positioned in the center of a 6" wafer. The Etch profile is more angled.
Dose test with the doses (J/m2): 200, 210, 220, 230, 240, 250, 270, 280
The aim was to get good line for 400nm pitch/200nm lines
<gallery caption="400nm pitch 200 nm lines" perrow="5" widths="200px" heights="150px">


Image:dose200_no2_22.jpg |200 J/m2 400nm/268nm
*Removing the H2 from the recipe to get less redeposition at lower platen power (200W), EM:02/30A. Se result below. This gave significantly lower etch rate and no etching in the smallest openings.
Image:dose210_no2_15.jpg |210 J/m2 400nm/239nm
Image:dose220_no2_13.jpg |220 J/m2 400nm/208nm
Image:dose230_no2_11.jpg |230 J/m2 400nm/209nm
Image:dose240_no2_05.jpg |240 J/m2 400nm/215nm
Image:dose250_no2_11.jpg |250 J/m2 400nm/207nm
Image:dose260_no2_18.jpg |260 J/m2 400nm/188nm
Image:dose270_no2_24.jpg |270 J/m2 400nm/155nm
Image:dose280_no1_15.jpg |280 J/m2 400nm/0nm


<gallery caption="Recipe name: SiO2_res, Recipe no. 10+EM+edit coils: C09975 coil_2500W, platen:200W, EM:02/30A, Pressure:8.8mTorr, C4F8:25.6sccm, He:448.7sccm, H2:0sccm, 3:56 min " perrow="5">
File:C09975_00.jpg
File:C09975_02.jpg
File:C09975_03.jpg
File:C09975_04.jpg
File:C09975_05.jpg
</gallery>
</gallery>


<gallery caption="1000nm pitch 500 nm lines" perrow="3" widths="200px" heights="150px">
<br clear="all"/>
 
 


Image:dose210_no2_17.jpg |210 J/m2 1000nm/581nm
==SiO2 etch with Cr mask==
Image:dose230_no2_12.jpg |230 J/m2 1000nm/517nm
{{CC-bghe2}} <br>
Image:dose240_no2_03.jpg |240 J/m2 1000nm/518nm
*[[/Cr mask|More tests with Cr mask]]
Image:dose250_no2_09.jpg |250 J/m2 1000nm/510nm
Image:dose260_no2_15.jpg |260 J/m2 1000nm/493nm
Image:dose270_no2_22.jpg |270 J/m2 1000nm/494nm


===SiO2 etch with Cr mask 100 nm and with 500 nm for the resist for the Cr etch===
Barc etch and Cr etch were done in ICP metal using end point detection. The sample was a full 6" wafer
<gallery caption="SiO2_res_10 2x5:00 min with 3 min TDESC clean in between 100 nm Cr mask, with 500 nm resist" widths="200px" heights="200px" perrow="6">
File:C041630_center_07.jpg
File:C041630_center_08.jpg
File:C041630_center_09.jpg
File:C041630_center_10.jpg
File:C041630_center_11.jpg
File:C041630_center_22.jpg
</gallery>
<gallery widths="200px" heights="200px" perrow="6">
File:C041630_center_02.jpg
File:C041630_center_03.jpg
File:C041630_center_04.jpg
File:C041630_center_05.jpg
File:C041630_center_06.jpg
</gallery>
</gallery>




==Testing with electromagnetic coils==
<gallery caption="SiO2_res_10 5:00 min 100 nm Cr mask, with 500 nm resist, resist/Cr stripped after etch in plasma asher 35min" widths="250px" heights="250px" perrow="4">
File:S0411376_profile_20.jpg| 200nm/400nm
File:S0411376_profile_13.jpg|250nm/500nm
File:S0411376_profile_14.jpg| 400nm/800nm
File:S0411376_profile_15.jpg|500nm/1000nm
File:S0411376_profile_17.jpg|1000nm/2000nm
File:S0411376_profile_18.jpg|2000nm/4000nm
 
</gallery>
 
===Testing with electromagnetic coils /Cr mask===
{{CC-bghe2}} <br>
{{CC-bghe2}} <br>


When testing with decreased platen power on the SiO2_10 standard recipe the uniformity got very bad. I then tested with the electromagnetics coil to see if that could affect the uniformity. There is and outer coil that can be varied between 0 and 10A and an inner coil that can be varied between 0 and 30 A. The first tests were don on Si/SiO2(1µm) without pattern and measured on the ellipsometer.  
 
When testing with decreased platen power on the SiO2_10 standard recipe the uniformity got very bad. I then tested with the electromagnetics coil to see if that could affect the uniformity. There is an outer coil that can be varied between 0 A and 10 A and an inner coil that can be varied between 0 A and 30 A. The first tests were done on Si/SiO2(1µm) without pattern and measured on the ellipsometer.  
{| border="2" cellspacing="2" cellpadding="3"  
{| border="2" cellspacing="2" cellpadding="3"  
!Parameter
!Parameter
Line 97: Line 123:


|-
|-
|Electromagnetic coils 'outer coil'/'inner coil'
|Electromagnetic coils (EM) 'outer coil' / 'inner coil'
|'0-10'A/'0-30'A
|'0-10 A' / '0-30 A'


|-
|-
Line 104: Line 130:


<gallery caption="EM tests" perrow="3" widths="400px" heights="300px">
<gallery caption="EM tests" perrow="3" widths="400px" heights="300px">
File:Contour Plot Y15 EM_0_0.JPG
File:Contour Plot Y15 EM_0_0.JPG| Etch time: 2 min, Average etch rate: 100.2 nm/min, range:+-55.1% 
File:Contour Plot Y16 EM_10_30.JPG
File:Contour Plot Y16 EM_10_30.JPG|Etch time: 2 min, Average etch rate: 100.5 nm/min, range:+-32.6% 
File:Contour Plot Y27 EM_10_0.JPG
File:Contour Plot Y27 EM_10_0.JPG|Etch time: 2 min, Average etch rate: 100.8 nm/min, range:+-50.8% 
File:Contour Plot Y26 EM_0_30.JPG
File:Contour Plot Y26 EM_0_30.JPG|Etch time: 2 min, Average etch rate: 203.8 nm/min, range:+-6.1% 
File:Contour Plot Y29 EM_2_30.JPG
File:Contour Plot Y29 EM_2_30.JPG|Etch time: 2 min, Average etch rate: 186.2 nm/min, range:+-3.2% 
File:Contour Plot patterned wafer EM_2_30.JPG
File:Contour Plot patterned wafer EM_2_30.JPG| Etch time: 6 min on patterned wafer with different measurement points, <100 nm Cr mask is still on, EM_2/30, Average etch rate: 207-223 nm/min depending on how much Cr mask is left, range:+-2.3% 
</gallery>
 
<gallery caption="EM tests with Cr mask on full wafer 6 min etch" perrow="3" widths="400px" heights="300px">
File:C09721_center_05.jpg
File:C09721_center_07.jpg
File:C09721_center_10.jpg
File:C09721_center_18.jpg
File:C09721_center_21.jpg
File:C09721_center_22.jpg
</gallery>
 
==SiO2 Etch using aSi as masking material==
 
{{CC-bghe2}} <br>
I was starting up development of SiO2 etch using aSi as masking material. This is on pause because the results did not look promishing on high aspect ratio structures wit DUV pattern due to large faceting on the aSi mask. I turned to Cr mask instead  <br>
The samples I use are:
*6" Si afters with oxide (2µm),
*aSi (~300nm),
*Neg. DUV reist (~60nm barc, ~350 nm resist)
*Reticle: Danchip/Triple-D
*Dose 230 J/m2
First I need to make sure that the resist work for pattering the aSi layer is good. If the resist is not good the final etch will also not be good.
 
===DUV optimization===
Dose test with the doses (J/m2): 200, 210, 220, 230, 240, 250, 270, 280
The aim was to get good line for 400nm pitch/200nm lines
<gallery caption="400nm pitch 200 nm lines" perrow="5" widths="200px" heights="150px">
 
Image:dose200_no2_22.jpg |200 J/m2 400nm/268nm
Image:dose210_no2_15.jpg |210 J/m2 400nm/239nm
Image:dose220_no2_13.jpg |220 J/m2 400nm/208nm
Image:dose230_no2_11.jpg |230 J/m2 400nm/209nm
Image:dose240_no2_05.jpg |240 J/m2 400nm/215nm
Image:dose250_no2_11.jpg |250 J/m2 400nm/207nm
Image:dose260_no2_18.jpg |260 J/m2 400nm/188nm
Image:dose270_no2_24.jpg |270 J/m2 400nm/155nm
Image:dose280_no1_15.jpg |280 J/m2 400nm/0nm
 
</gallery>
 
<gallery caption="1000nm pitch 500 nm lines" perrow="3" widths="200px" heights="150px">
 
Image:dose210_no2_17.jpg |210 J/m2 1000nm/581nm
Image:dose230_no2_12.jpg |230 J/m2 1000nm/517nm
Image:dose240_no2_03.jpg |240 J/m2 1000nm/518nm
Image:dose250_no2_09.jpg |250 J/m2 1000nm/510nm
Image:dose260_no2_15.jpg |260 J/m2 1000nm/493nm
Image:dose270_no2_22.jpg |270 J/m2 1000nm/494nm
 
</gallery>
</gallery>

Latest revision as of 11:45, 7 April 2026

SiO2 Etch using resist as masking material

Unless otherwise stated, all content in this section was done by Berit Herstrøm, DTU Nanolab
I have do some development of a SiO2 etch with resist as masking material. I have found this fairly good recipe. For now it is the standard SiO2 etch recipes but I might change the "Standard recipe" a a later time if I find a better one. If you need to etch deeper than 1 micrometer then I advise you to split the etch in several runs with O2 cleans in between (3min TDESC Clean) or else it seems like the the etch rate is going down over time.


Uniformity results with SiO2_res_10

Etched for 3min56s, average etch rate: 250 nm/min +- 2.9%


Results with SiO2_res_10 and with with the electro magnets on

The SiO2:res_10 recipe was tested with the electromagnets on but it seems to no no good for the results.

Etched with EM:02/30 for 2min, average etch rate: 275 nm/min +- 4.5%. The electro magnets changed the uniformity pattern and made it a bit worse


Using the electromagnetic coil on the recipe SiO2_res_10 gave higher etch rate on this chip, which is positioned in the center of a 6" wafer. The Etch profile is more angled.

  • Removing the H2 from the recipe to get less redeposition at lower platen power (200W), EM:02/30A. Se result below. This gave significantly lower etch rate and no etching in the smallest openings.



SiO2 etch with Cr mask

Unless otherwise stated, all content in this section was done by Berit Herstrøm, DTU Nanolab

SiO2 etch with Cr mask 100 nm and with 500 nm for the resist for the Cr etch

Barc etch and Cr etch were done in ICP metal using end point detection. The sample was a full 6" wafer


Testing with electromagnetic coils /Cr mask

Unless otherwise stated, all content in this section was done by Berit Herstrøm, DTU Nanolab


When testing with decreased platen power on the SiO2_10 standard recipe the uniformity got very bad. I then tested with the electromagnetics coil to see if that could affect the uniformity. There is an outer coil that can be varied between 0 A and 10 A and an inner coil that can be varied between 0 A and 30 A. The first tests were done on Si/SiO2(1µm) without pattern and measured on the ellipsometer.

Parameter Recipe name: no 10 with lower platen power
Coil Power [W] 2500
Platen Power [W] 200
Platen temperature [oC] 20
H2 flow [sccm] 25.6
C4F8 flow [sccm] 25.6
He flow [sccm] 448.7
Pressure Fully open APC valve (8-9 mTorr)
Electromagnetic coils (EM) 'outer coil' / 'inner coil' '0-10 A' / '0-30 A'

SiO2 Etch using aSi as masking material

Unless otherwise stated, all content in this section was done by Berit Herstrøm, DTU Nanolab
I was starting up development of SiO2 etch using aSi as masking material. This is on pause because the results did not look promishing on high aspect ratio structures wit DUV pattern due to large faceting on the aSi mask. I turned to Cr mask instead
The samples I use are:

  • 6" Si afters with oxide (2µm),
  • aSi (~300nm),
  • Neg. DUV reist (~60nm barc, ~350 nm resist)
  • Reticle: Danchip/Triple-D
  • Dose 230 J/m2

First I need to make sure that the resist work for pattering the aSi layer is good. If the resist is not good the final etch will also not be good.

DUV optimization

Dose test with the doses (J/m2): 200, 210, 220, 230, 240, 250, 270, 280 The aim was to get good line for 400nm pitch/200nm lines