Jump to content

Specific Process Knowledge/Lithography/CSAR: Difference between revisions

Thope (talk | contribs)
Elelop (talk | contribs)
No edit summary
 
(2 intermediate revisions by one other user not shown)
Line 1: Line 1:


Simple e-beam pattern in this resist has been tested, the results showed on this page. If you have questions to the process or wish to use this e-beam resist, please contact [mailto:lithography@nanolab.dtu.dk lithography] at DTU Nanolab.
Simple e-beam pattern in this resist has been tested, the results showed on this page. If you have questions to the process or wish to use this e-beam resist, please contact [mailto:lithography@nanolab.dtu.dk lithography] at DTU Nanolab.


== Spin Curves ==
== Spin Curves ==
Line 190: Line 186:
|549
|549
|-
|-
|}
|}


<br>
<br>
<br>


== Contrast Curve ==
== Contrast Curve ==
Line 234: Line 225:
{| style="border: none; border-spacing: 0; margin: 1em auto; text-align: center;"
{| style="border: none; border-spacing: 0; margin: 1em auto; text-align: center;"
|-
|-
| [[image:ContrastCurvesCSAR_March2016_log.png|800px]]
| [[image:ContrastCurvesCSAR_March2016_log.png|600px]]
|-  
|-  
| colspan="1" style="text-align:center;|
| colspan="1" style="text-align:center;|
Line 240: Line 231:
|}
|}


[[File:ContrastCurvesCSAR_March2016_log.png|600px]]
==Dose to size==
 
Small features need a comparatively higher dose then big features and hence it can be useful to map out the dose and size dependency. Below is a set of cross sectional images of 100, 50 and 20 nm lines written 500, 250 and 180 nm resist at doses from 200 to 600 µC/cm<sup>2</sup>.
==Cross section dose lines==


{| style="border: none; border-spacing: 0; margin: 1em auto; text-align: center;"
{| style="border: none; border-spacing: 0; margin: 1em auto; text-align: center;"
Line 265: Line 255:
|-
|-
| colspan="1" style="text-align:center;|
| colspan="1" style="text-align:center;|
Cross section SEM images of 500 nm AR-P 6200.09 exposed at 200-600 µC/cm<sup>2</sup>. Top image is 100 nm lines, center image is 50 nm lines, bottom image is 20 nm lines. Au coated for SEM imaging.
Cross section SEM images of 250 nm AR-P 6200.09 exposed at 200-600 µC/cm<sup>2</sup>. Top image is 100 nm lines, center image is 50 nm lines, bottom image is 20 nm lines. Au coated for SEM imaging.
|}
|}


Line 277: Line 267:
|-  
|-  
| colspan="1" style="text-align:center;|
| colspan="1" style="text-align:center;|
Cross section SEM images of 250 nm AR-P 6200.09 exposed at 200-600 µC/cm<sup>2</sup>. Top image is 100 nm lines, center image is 50 nm lines, bottom image is 20 nm lines. Au coated for SEM imaging.
Cross section SEM images of 180 nm AR-P 6200.09 exposed at 200-600 µC/cm<sup>2</sup>. Top image is 100 nm lines, center image is 50 nm lines, bottom image is 20 nm lines. Au coated for SEM imaging.
|}
|}