Simple e-beam pattern in this resist has been tested, the results showed on this page. If you have questions to the process or wish to use this e-beam resist, please contact [mailto:lithography@nanolab.dtu.dk lithography] at DTU Nanolab.
Simple e-beam pattern in this resist has been tested, the results showed on this page. If you have questions to the process or wish to use this e-beam resist, please contact [mailto:lithography@nanolab.dtu.dk lithography] at DTU Nanolab.


== Spin Curves ==
== Spin Curves ==
Line 190: Line 186:
|549
|549
|-
|-
|}
|}


<br>
<br>
<br>


== Contrast Curves ==
== Contrast Curve ==


=== CSAR 6200.09 ===
=== CSAR 6200.09 ===


100 nm lines in both ~70 nm and ~188 nm thick CSAR has been developed with AR-600-546 (standard CSAR developer) at room temperature.  
100 nm lines in both ~70 nm and ~188 nm thick CSAR has been developed with AR-600-546 (standard CSAR developer) at room temperature to provide the following contrast curves.


{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;"  style="width: 95%"
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;"  style="width: 95%"
Line 232: Line 223:
|}
|}


[[File:ContrastCurvesCSAR_March2016_log.png|600px]]
{| style="border: none; border-spacing: 0; margin: 1em auto; text-align: center;"
|-
| [[image:ContrastCurvesCSAR_March2016_log.png|600px]]
|-
| colspan="1" style="text-align:center;|
AR-P 6200 contrast curves.
|}
 
==Dose to size==
Small features need a comparatively higher dose then big features and hence it can be useful to map out the dose and size dependency. Below is a set of cross sectional images of 100, 50 and 20 nm lines written 500, 250 and 180 nm resist at doses from 200 to 600 µC/cm<sup>2</sup>.
 
{| style="border: none; border-spacing: 0; margin: 1em auto; text-align: center;"
|-
| [[image:thope240214_lines_100_06.png|1200px]]
|-
| [[image:thope240214_lines_50_11.png|1200px]]
|-
| [[image:thope240214_lines_20_13.png|1200px]]
|-
| colspan="1" style="text-align:center;|
Cross section SEM images of 500 nm AR-P 6200.09 exposed at 200-600 µC/cm<sup>2</sup>. Top image is 100 nm lines, center image is 50 nm lines, bottom image is 20 nm lines. Au coated for SEM imaging.
|}
 
{| style="border: none; border-spacing: 0; margin: 1em auto; text-align: center;"
|-
| [[image:thope240214_lines250_100nm.png|1200px]]
|-
| [[image:thope240214_lines250_50nm.png|1200px]]
|-
| [[image:thope240214_lines250_20nm.png|1200px]]
|-
| colspan="1" style="text-align:center;|
Cross section SEM images of 250 nm AR-P 6200.09 exposed at 200-600 µC/cm<sup>2</sup>. Top image is 100 nm lines, center image is 50 nm lines, bottom image is 20 nm lines. Au coated for SEM imaging.
|}
 
{| style="border: none; border-spacing: 0; margin: 1em auto; text-align: center;"
|-
| [[image:thope240214_lines180_100_29.png|1200px]]
|-
| [[image:thope240214_lines180_50_31.png|1200px]]
|-
| [[image:thope240214_lines180_20_33.png|1200px]]
|-
| colspan="1" style="text-align:center;|
Cross section SEM images of 180 nm AR-P 6200.09 exposed at 200-600 µC/cm<sup>2</sup>. Top image is 100 nm lines, center image is 50 nm lines, bottom image is 20 nm lines. Au coated for SEM imaging.
|}


=== CSAR 6200.18 ===
=== CSAR 6200.18 ===
Line 291: Line 327:
Some users have reported residues and residual layers when using ZED N-50 on CSAR and vice verca, hence we recommend to use AR 600-546 or AR 600-548 (3 times stronger) to develop CSAR and not ZED N-50.
Some users have reported residues and residual layers when using ZED N-50 on CSAR and vice verca, hence we recommend to use AR 600-546 or AR 600-548 (3 times stronger) to develop CSAR and not ZED N-50.


When this is said some users still observe residues when using AR 600-546, "'''All resist'''" have recommended to use 3-5s, dip in pure MIBK to remove residues.  
When this is said some users still observe residues when using AR 600-546, the producer "'''All resist GMBH'''" have recommended to use 3-5s, dip in pure MIBK to remove residues.  
   
   
 
AR 600 546 will dissolve different plastic materials, hence never use it on PS compounds.


<br clear="all"/>
<br clear="all"/>
== Dosetests ==
So far (September 2014) three wafers with CSAR have been e-beam exposed with dosetests and inspected in SEM. Thickness of resist, e-beam dose and development time has been changed somewhat from wafer to wafer:
style = "border-radius: 6px; border: 3px solid #000000;
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;" style="width: 90%; style = "border-radius: 6px; border: 2px solid #000000;"
|-
|-
|-style="background:Black; text-align:left; color:White"
!rowspan="2"|Process
!rowspan="2"|Equipment
!colspan="3"|Parameters
|-
|-
|-style="background:Black; text-align:left; color:White"
!width="300"|6.13
!width="300"|4.09
!width="300"|3.05
|-
|-
|-style="background:WhiteSmoke; color:black"
|Resist
|Fumehood D-3
|'''Resist:''' AR-P 6200/2 diluted 1:1 in anisole (Bottled opened 16-06-2014 TIGRE)
|'''Resist:''' AR-P 6200/2 diluted 1:1 in anisole (Bottled opened 16-06-2014 TIGRE)
|'''Resist:''' AR-P 6200/2
|-
|-style="background:WhiteSmoke; color:black"
|Spin Coat
|Spin Coater LabSpin A-5
|'''Spin:''' 1 min @ 6000 rpm,<br /> '''softbake:''' 1 min @ 150 degC, <br />'''thickness:''' ~50nm <br />(27-08-2014 TIGRE)
|'''Spin:''' 1 min @ 5000 rpm,<br /> '''softbake:''' 2 min @ 150 degC, <br />'''thickness:''' ~53nm <br />(16-06-2014 TIGRE)
|'''Spin:''' 1 min @ 6000 rpm,<br /> '''softbake:''' 5 min @ 150 degC, <br />'''thickness:''' ~143nm <br />(09-04-2014 TIGRE)
|-
|-
|-style="background:WhiteSmoke; color:black"
|E-beam exposure
|JEOL 9500 E-2
|'''Condition file:''' 0.2nA_ap5,<br /> '''doses:''' 180-420 muC/cm2,<br /> '''Shot pitch:''' 7-27 nm,<br /> '''PEC:''' no <br />(27-08-2014 TIGRE)
|'''Condition file:''' 0.2nA_ap5,<br /> '''doses:''' 207-242 muC/cm2,<br /> '''Shot pitch:''' 5 nm,<br /> '''PEC:''' no <br />(02-07-2014 TIGRE)
|'''Condition file:''' 2nA_ap5,<br /> '''doses:''' 207-242 muC/cm2,<br /> '''Shot pitch:''' 5 nm,<br /> '''PEC:''' no <br />(10-04-2014 TIGRE)
|-
|-
|-style="background:WhiteSmoke; color:black"
|Develop
|Fumehood D-3
|'''Developer:''' SX-AR 600-54/6,<br /> '''time:''' 30 sec,<br /> '''Rinse:''' 30 sec in IPA<br /> (28-08-2014 TIGRE)
|'''Developer:''' SX-AR 600-54/6,<br /> '''time:''' 60 sec,<br /> '''Rinse:''' 30 sec in IPA<br /> (08-07-2014 TIGRE)
|'''Developer:''' SX-AR 600-54/6,<br /> '''time:''' 60 sec,<br /> '''Rinse:''' 60 sec in IPA<br /> (April/May-2014 TIGRE)
|-
|-
|-style="background:WhiteSmoke; color:black"
|Sputter Coat (please contact [mailto:ramona.mateiu@cen.dtu.dk Ramona Valentina Mateiu] for information )
|Cressington 208HR, DTU CEN
|3-5 nm Pt, sputtering, (29-08-2014 TIGRE)
|3-5 nm Pt, sputtering (09-07-2014 TIGRE)
|3-5 nm Pt, sputtering (22-05-2014 TIGRE)
|-
|-
|-style="background:WhiteSmoke; color:black"
|Characterization
|Zeiss SEM Supra 60VP, D-3
|'''Acc voltage:''' 3 kV, '''WD:''' < 4mm, <br />conducting tape close to pattern (29-08-2014 TIGRE)
|'''Acc voltage:''' 3 kV, '''WD:''' < 4mm, <br />conducting tape close to pattern (09-07-2014 TIGRE)
|'''Acc voltage:''' 2 kV, '''WD:''' < 4mm, <br />conducting tape close to pattern (06-06-2014 TIGRE)
|-
|}
=== SEM inspection ===
{| class = "collapsible collapsed"  width=100% style = "border-radius: 6px; -moz-border-radius: 10px; -webkit-border-radius: 10px; -khtml-border-radius: 10px; -icab-border-radius: 10px; -o-border-radius: 10px; border: 3px solid #000000;"
! width=15% |
! colspan="7" width=85% | SEM inspection of wafer 6.13, 100 nm exposed pattern, shot pitch 7 nm
|-
|-
! 300 [muC/cm2]
| [[File:6_13_100nm_300_shot14.png|200px]]
| [[File:6_13_100nm_300_shot14_Lines.png|200px]]
| [[File:6_13_100nm_300_shot14_Holes.png|200px]]
| [[File:6_13_100nm_300_shot14_Holes2.png|200px]]
| [[File:6_13_100nm_300_shot14_Pillars.png|200px]]
| [[File:6_13_100nm_300_shot14_Test.png|200px]]
! ACHK NOT READY
|-
|}
{| class = "collapsible collapsed"  width=100% style = "border-radius: 6px; border: 3px solid #000000;"
! width=15% |
!colspan="7" width=85%|  SEM inspection of wafer 6.13, 50 nm exposed pattern, shot pitch 7 nm
|-
|-
! 270 [muC/cm2]
| [[File:6_13_50nm_270_shot14.png|200px]]
| [[File:6_13_50nm_270_shot14_Lines.png|200px]]
| [[File:6_13_50nm_270_shot14_Holes.png|200px]]
| [[File:6_13_50nm_270_shot14_Pillars.png|200px]]
| [[File:6_13_50nm_270_shot14_Holes2.png|200px]]
! ACHK NOT READY
|-
|-
! 300 [muC/cm2]
| [[File:6_13_50nm_300_shot14.png|200px]]
| [[File:6_13_50nm_300_shot14_Lines.png|200px]]
| [[File:6_13_50nm_300_shot14_Holes.png|200px]]
| [[File:6_13_50nm_300_shot14_Pillars.png|200px]]
| [[File:6_13_50nm_300_shot14_Holes2.png|200px]]
! ACHK NOT READY
|-
|}
{| class = "collapsible collapsed"  width=100% style = "border-radius: 6px; -moz-border-radius: 10px; -webkit-border-radius: 10px; -khtml-border-radius: 10px; -icab-border-radius: 10px; -o-border-radius: 10px; border: 3px solid #000000;"
! width=15% |
!colspan="7" width=85%| SEM inspection of wafer 6.13, 30 nm exposed pattern, shot pitch 7 nm
|-
|-
! 270 [muC/cm2]
| [[File:6_13_30nm_270_shot14.png|200px]]
| [[File:6_13_30nm_270_shot14_Lines.png|200px]]
| [[File:6_13_30nm_270_shot14_Holes.png|200px]]
| [[File:6_13_30nm_270_shot14_Pillars.png|200px]]
! ACHK NOT READY
|-
|-
! 300 [muC/cm2]
| [[File:6_13_30nm_300_shot14.png|200px]]
| [[File:6_13_30nm_300_shot14_Lines.png|200px]]
| [[File:6_13_30nm_300_shot14_Holes.png|200px]]
| [[File:6_13_30nm_300_shot14_Pillars.png|200px]]
! ACHK NOT READY
|-
|}
{| class = "collapsible collapsed"  width=100% style = "border-radius: 6px; -moz-border-radius: 10px; -webkit-border-radius: 10px; -khtml-border-radius: 10px; -icab-border-radius: 10px; -o-border-radius: 10px; border: 3px solid #000000;"
! width=15%|
! colspan="4"|  SEM inspection of wafer 6.13, 20 nm exposed pattern, shot pitch 7 nm
|-
|-
! 270 [muC/cm2]
| [[File:6_13_20nm_270_shot14.png|200px]]
| [[File:6_13_20nm_270_shot14_Lines.png|200px]]
| ACHK NOT READY
|-
|-
! 300 [muC/cm2]
| [[File:6_13_20nm_300_shot14.png|200px]]
| [[File:6_13_20nm_300_shot14_Lines.png|200px]]
| ACHK NOT READY
|-
|}
{| class = "collapsible collapsed"  width=100% style = "border-radius: 6px; -moz-border-radius: 10px; -webkit-border-radius: 10px; -khtml-border-radius: 10px; -icab-border-radius: 10px; -o-border-radius: 10px; border: 3px solid #000000;"
! width=15%|
! colspan="6"|  SEM inspection of wafer 4.09, 50 nm exposed pattern, shot pitch 5 nm
|-
! 230 [muC/cm2]
| [[File:53nmCSAR50nmOverviewBasedose.png|250px]]
| [[File:53nmCSAR50nmLinesBasedose.png|250px]]
| [[File:53nmCSAR50nmHolesBasedose.png|250px]]
| [[File:53nmCSAR50nmPillarsBasedose.png|250px]]
| [[File:53nmCSAR50nmTestBasedose.png|250px]]
|}
{| class = "collapsible collapsed"  width=100% style = "border-radius: 6px; -moz-border-radius: 10px; -webkit-border-radius: 10px; -khtml-border-radius: 10px; -icab-border-radius: 10px; -o-border-radius: 10px; border: 3px solid #000000;"
! width=15%|
! colspan="4"|  SEM inspection of wafer 4.09, 30 nm exposed pattern, shot pitch 5 nm
|-
|-
! 219 [muC/cm2]
| [[File:53nmCSAR30nmOverviewBasedose-5%.png|250px]]
| [[File:53nmCSAR30nmLinesBasedose-5%.png|250px]]
| [[File:30nmShot10.png|250px]]
|-
|-
! 230 [muC/cm2]
| [[File:53nmCSAR30nmOverviewBasedose.png|250px]]
| [[File:53nmCSAR30nmLinesBasedose.png|250px]]
|
|-
|-
! 242 [muC/cm2]
| [[File:53nmCSAR30nmOverviewBasedose+5%.png|250px]]
| [[File:53nmCSAR30nmLinesBasedose+5%.png|250px]]
|
|-
|}
{| class = "collapsible collapsed"  width=100% style = "border-radius: 6px; -moz-border-radius: 10px; -webkit-border-radius: 10px; -khtml-border-radius: 10px; -icab-border-radius: 10px; -o-border-radius: 10px; border: 3px solid #000000;"
! width=15%|
! colspan="4"|  SEM inspection of wafer 4.09, 20 nm exposed pattern, shot pitch 5 nm
|-
|-
! 242 [muC/cm2]
| [[File:53nmCSAR20nmOverviewBasedose+5%.png|220px]]
| [[File:53nmCSAR20nmLines2Basedose+5%.png|220px]]
|
|-
|-
! 253 [muC/cm2]
| [[File:53nmCSAR20nmOverviewBasedose+10%.png|220px]]
| [[File:53nmCSAR20nmLinesBasedose+10%.png|220px]]
|
|-
|}
{| class = "collapsible collapsed"  width=100% style = "border-radius: 6px; -moz-border-radius: 10px; -webkit-border-radius: 10px; -khtml-border-radius: 10px; -icab-border-radius: 10px; -o-border-radius: 10px; border: 3px solid #000000;"
! width=15%|
! colspan="4"|  SEM inspection of wafer 3.05, 50 nm exposed pattern, shot pitch 5 nm
|-
|-
! 219 [muC/cm2]
| [[File:CSAR50nmoverview-5%.png|270px]]
| [[File:CSAR50nmlines-5%.png|270px]]
|
|-
|-
! 230 [muC/cm2]
| [[File:CSAR50nmoverview.png|270px]]
| [[File:CSAR50nmlines.png|270px]]
|
|-
|-
! 242 [muC/cm2]
| [[File:CSAR50nmoverview+5%.png|270px]]
| [[File:CSAR50nmlines+5%.png|270px]]
|
|-
|}
{| class = "collapsible collapsed"  width=100% style = "border-radius: 6px; -moz-border-radius: 10px; -webkit-border-radius: 10px; -khtml-border-radius: 10px; -icab-border-radius: 10px; -o-border-radius: 10px; border: 3px solid #000000;"
! width=15%|
! colspan="4"|  SEM inspection of wafer 3.05, 30 nm exposed pattern, shot pitch 5 nm
|-
|-
! 219 [muC/cm2]
| [[File:CSAR30nmoverview-5%.png|270px]]
| [[File:CSAR30nmlines-5%.png|270px]]
|
|-
|-
! 230 [muC/cm2]
| [[File:CSAR30nmoverview.png|270px]]
| [[File:CSAR30nmlines.png|270px]]
|
|-
|-
! 242 [muC/cm2]
| [[File:CSAR30nmoverview+5%.png|270px]]
| [[File:CSAR30nmlines+5%.png|270px]]
|
|-
|}
{| class = "collapsible collapsed"  width=100% style = "border-radius: 6px; -moz-border-radius: 10px; -webkit-border-radius: 10px; -khtml-border-radius: 10px; -icab-border-radius: 10px; -o-border-radius: 10px; border: 3px solid #000000;"
! width=15%|
! colspan="4"|  SEM inspection of wafer 3.05, 20 nm exposed pattern, shot pitch 5 nm
|-
|-
! 230 [muC/cm2]
| [[File:CSAR20nmoverview.png|280px]]
|
|-
|-
! 242 [muC/cm2]
| [[File:CSAR20nmoverview+5%.png|280px]]
|
|-
|-
! 253 [muC/cm2]
| [[File:CSAR20nmoverview+10%.png|280px]]
|
|-
|}


== Etch Tests ==