Simple e-beam pattern in this resist has been tested, the results showed on this page. If you have questions to the process or wish to use this e-beam resist, please contact [mailto:lithography@nanolab.dtu.dk lithography] at DTU Nanolab.
Simple e-beam pattern in this resist has been tested, the results showed on this page. If you have questions to the process or wish to use this e-beam resist, please contact Tine Greibe at tigre@danchip.dtu.dk.
|Disposal pipette used; clean by N2-gun before use. Use approximately 1.5 ml per 4" wafer, never use a pipette twice. Softbake is not a crucial step, see e-mail correspondence with AllResist [[media:Softbake CSAR.pdf|here]].
|2-3 kV, shortest working distance possible, chip mounted with Al tape
|For dosepattern SEM inspection: the wafers are diced into smaller pieces and sputter coated with Pt at DTU CEN before SEM inspection; please contact [mailto:ramona.mateiu@cen.dtu.dk Ramona Valentina Mateiu] for further information.
| Residues: After a dry etch, residues are very easily observed by SEM inspection. This particular trench was e-beam patterned at a too low dose. Residues are recommended removed by optimising dose and developing, not by plasma ashing, since our plasma ashers in the cleanroom are 'dirty' and most likely generate particles on the substrate.
|}
== Spin Curves ==
== Spin Curves ==
Line 148:
Line 7:
The thickness is measured on VASE Ellipsometer using a simple Cauchy model for a transparent polymer on Si. The measurements are performed at one incidence angle (70 degrees) only. 9 points on each 4" wafer has been measured; the standard deviation thus representing the homogeinity of the film on the 4" wafers.
The thickness is measured on VASE Ellipsometer using a simple Cauchy model for a transparent polymer on Si. The measurements are performed at one incidence angle (70 degrees) only. 9 points on each 4" wafer has been measured; the standard deviation thus representing the homogeinity of the film on the 4" wafers.
Please be aware that I have experienced a somewhat large thickness deviation (5-8 %) depending on the amount of resist applied to the wafer before spin coating.
Around 2 ml of resist per wafer has been used when fabricating these curves. If you use less than 2 ml, the thickness of the final resist might be smaller than reported here.
Line 160:
Line 19:
|-
|-
|-style="background:Blue; color:White"
|-style="background:#00308F; color:White"
!colspan="7"|AllResist AR-P 6200.09 (> 2ml per 4" wafer) spinning on Spin Coater: Manual LabSpin A-5, TIGRE, 09-04-2014. Softbake 5 min @ 150 degC.
!colspan="7"|AllResist AR-P 6200.09 (> 2ml per 4" wafer) spinning on Spin Coater: Manual LabSpin A-5, TIGRE, 09-04-2014. Softbake 5 min @ 150 degC.
|-
|-
Line 327:
Line 186:
|549
|549
|-
|-
|}
|}
<br>
<br>
<br>
== Contrast Curves ==
== Contrast Curve ==
=== CSAR 6200.09 ===
=== CSAR 6200.09 ===
100 nm lines in both ~70 nm and ~188 nm thick CSAR has been developed with AR-600-546 (standard CSAR developer) at room temperature.
100 nm lines in both ~70 nm and ~188 nm thick CSAR has been developed with AR-600-546 (standard CSAR developer) at room temperature to provide the following contrast curves.
Small features need a comparatively higher dose then big features and hence it can be useful to map out the dose and size dependency. Below is a set of cross sectional images of 100, 50 and 20 nm lines written 500, 250 and 180 nm resist at doses from 200 to 600 µC/cm<sup>2</sup>.
Cross section SEM images of 500 nm AR-P 6200.09 exposed at 200-600 µC/cm<sup>2</sup>. Top image is 100 nm lines, center image is 50 nm lines, bottom image is 20 nm lines. Au coated for SEM imaging.
Cross section SEM images of 250 nm AR-P 6200.09 exposed at 200-600 µC/cm<sup>2</sup>. Top image is 100 nm lines, center image is 50 nm lines, bottom image is 20 nm lines. Au coated for SEM imaging.
Cross section SEM images of 180 nm AR-P 6200.09 exposed at 200-600 µC/cm<sup>2</sup>. Top image is 100 nm lines, center image is 50 nm lines, bottom image is 20 nm lines. Au coated for SEM imaging.
|}
=== CSAR 6200.18 ===
=== CSAR 6200.18 ===
Line 377:
Line 276:
[[File:CSAR 6200.18 developed with AR600546.png|right|400px]]
[[File:CSAR 6200.18 developed with AR600546.png|right|400px]]
|16-06-2016, Fumehood E-4, AR-600-546, rinsed in IPA 60s.
|16-06-2016, Fumehood E-4, AR-600-546, 30s/60s/90s, rinsed in IPA 60s.
|JUNE/JULY 2016 SEM Supra 2, 10 keV
|JUNE/JULY 2016 SEM Supra 2, 10 keV
|-
|-
Line 405:
Line 304:
|}
|}
<br clear="all"\>
<br clear="all"/>
=== Dark Erosion ===
=== Dark Erosion ===
Line 419:
Line 319:
<br clear="all" />
<br clear="all" />
== Dosetests ==
== Development ==
So far (September 2014) three wafers with CSAR have been e-beam exposed with dosetests and inspected in SEM. Thickness of resist, e-beam dose and development time has been changed somewhat from wafer to wafer:
Many resists can be developed in different developers, CSAR can be developed in: AR 600-546, AR 600-548, ZED N-50 and mix of MIBK and IPA among others.
|-style="background:WhiteSmoke; color:black"
|Resist
|Fumehood D-3
|'''Resist:''' AR-P 6200/2 diluted 1:1 in anisole (Bottled opened 16-06-2014 TIGRE)
|'''Resist:''' AR-P 6200/2 diluted 1:1 in anisole (Bottled opened 16-06-2014 TIGRE)
|'''Resist:''' AR-P 6200/2
|-
|-style="background:WhiteSmoke; color:black"
|Spin Coat
|Spin Coater LabSpin A-5
|'''Spin:''' 1 min @ 6000 rpm,<br /> '''softbake:''' 1 min @ 150 degC, <br />'''thickness:''' ~50nm <br />(27-08-2014 TIGRE)
|'''Spin:''' 1 min @ 5000 rpm,<br /> '''softbake:''' 2 min @ 150 degC, <br />'''thickness:''' ~53nm <br />(16-06-2014 TIGRE)
|'''Spin:''' 1 min @ 6000 rpm,<br /> '''softbake:''' 5 min @ 150 degC, <br />'''thickness:''' ~143nm <br />(09-04-2014 TIGRE)
Some users have reported residues and residual layers when using ZED N-50 on CSAR and vice verca, hence we recommend to use AR 600-546 or AR 600-548 (3 times stronger) to develop CSAR and not ZED N-50.
! width=15% |
! colspan="7" width=85% | SEM inspection of wafer 6.13, 100 nm exposed pattern, shot pitch 7 nm
When this is said some users still observe residues when using AR 600-546, the producer "'''All resist GMBH'''" have recommended to use 3-5s, dip in pure MIBK to remove residues.
AR 600 546 will dissolve different plastic materials, hence never use it on PS compounds.
! colspan="4"| SEM inspection of wafer 3.05, 20 nm exposed pattern, shot pitch 5 nm
|-
|-
! 230 [muC/cm2]
| [[File:CSAR20nmoverview.png|280px]]
|
|-
|-
! 242 [muC/cm2]
| [[File:CSAR20nmoverview+5%.png|280px]]
|
|-
|-
! 253 [muC/cm2]
| [[File:CSAR20nmoverview+10%.png|280px]]
|
|-
|}
== Etch Tests ==
== Etch Tests ==
Latest revision as of 15:50, 4 February 2026
Simple e-beam pattern in this resist has been tested, the results showed on this page. If you have questions to the process or wish to use this e-beam resist, please contact lithography at DTU Nanolab.
Spin Curves
The thickness is measured on VASE Ellipsometer using a simple Cauchy model for a transparent polymer on Si. The measurements are performed at one incidence angle (70 degrees) only. 9 points on each 4" wafer has been measured; the standard deviation thus representing the homogeinity of the film on the 4" wafers.
Around 2 ml of resist per wafer has been used when fabricating these curves. If you use less than 2 ml, the thickness of the final resist might be smaller than reported here.
AllResist AR-P 6200.09 (> 2ml per 4" wafer) spinning on Spin Coater: Manual LabSpin A-5, TIGRE, 09-04-2014. Softbake 5 min @ 150 degC.
Spin Speed [rpm]
Acceleration [1/s2]
Thickness [nm]
2000
4000
226
3000
4000
194
4000
4000
170
5000
4000
151
6000
4000
142
7000
4000
127
AllResist CSAR 6200.09 1:1 in anisole (< 2ml per 4" wafer), Spin Coater: Manual LabSpin A-5, TIGRE, 16-06-2014. Softbake 2 min @ 150 degC.
Spin Speed [rpm]
Acceleration [1/s2]
Thickness [nm]
2000
4000
84
3000
4000
67
4000
4000
59
5000
4000
53
6000
4000
49
AllResist CSAR 6200.18 (< 2ml per 4" wafer), Spin Coater: Manual Standard Resists, E-5, TIGRE, 15-06-2016. Softbake 2 min @ 180 degC.
Spin Speed [rpm]
Acceleration [1/s2]
Thickness [nm]
2000
2000
1003
3000
2000
809
4000
2000
721
5000
2000
639
6000
2000
586
7000
2000
549
Contrast Curve
CSAR 6200.09
100 nm lines in both ~70 nm and ~188 nm thick CSAR has been developed with AR-600-546 (standard CSAR developer) at room temperature to provide the following contrast curves.
CSAR Contrast Curve, Processed by TIGRE, FEB-MARCH 2016
Resist
Spin Coat
E-beam exposure
Development
Characterisation
CSAR AR-P6200.09 AllResist, CSAR AR-P6200.09 diluted 1:1 in Anisole
11-02-2016, Fumehood D-2, AR-600-546, rinsed in IPA 60s.
02-03-2016 AFM Icon, F-2, ScanAsyst in Air
AR-P 6200 contrast curves.
Dose to size
Small features need a comparatively higher dose then big features and hence it can be useful to map out the dose and size dependency. Below is a set of cross sectional images of 100, 50 and 20 nm lines written 500, 250 and 180 nm resist at doses from 200 to 600 µC/cm2.
Cross section SEM images of 500 nm AR-P 6200.09 exposed at 200-600 µC/cm2. Top image is 100 nm lines, center image is 50 nm lines, bottom image is 20 nm lines. Au coated for SEM imaging.
Cross section SEM images of 250 nm AR-P 6200.09 exposed at 200-600 µC/cm2. Top image is 100 nm lines, center image is 50 nm lines, bottom image is 20 nm lines. Au coated for SEM imaging.
Cross section SEM images of 180 nm AR-P 6200.09 exposed at 200-600 µC/cm2. Top image is 100 nm lines, center image is 50 nm lines, bottom image is 20 nm lines. Au coated for SEM imaging.
CSAR 6200.18
100 nm lines in ~900 nm thick CSAR has been developed with AR-600-546 (standard CSAR developer) at room temperature.
CSAR Contrast Curve, Processed by TIGRE, JUNE 2016
16-06-2016, Fumehood E-4, AR-600-546, 30s/60s/90s, rinsed in IPA 60s.
JUNE/JULY 2016 SEM Supra 2, 10 keV
Dark Erosion
Dark erosion has been measured on a un-exposed 4" wafer spin coated with CSAR 6200.18 to a thickness of approximately 549 nm. The resist thickness has been measured by VASE Ellipsometer before development, and after 3 minutes, 13 minutes, and 30 minutes of development in AR 600 546.
The graphs shows the measured thicknesses; the errorbars represents the standard deviations from the ellipsometric measurements. The average etch rate of CSAR is ~0.1 nm/min.
Development
Many resists can be developed in different developers, CSAR can be developed in: AR 600-546, AR 600-548, ZED N-50 and mix of MIBK and IPA among others.
CSAR and ZEP520A are in principle the same chemical, however the pretreatment (filtration and temperature control) can differ.
Some users have reported residues and residual layers when using ZED N-50 on CSAR and vice verca, hence we recommend to use AR 600-546 or AR 600-548 (3 times stronger) to develop CSAR and not ZED N-50.
When this is said some users still observe residues when using AR 600-546, the producer "All resist GMBH" have recommended to use 3-5s, dip in pure MIBK to remove residues.
AR 600 546 will dissolve different plastic materials, hence never use it on PS compounds.
Etch Tests
If you have wafers or chips with CSAR you would like to have tested, please send me an [email].
Chlorine versus flourine-based etches
We have experienced problems with removal of CSAR after chlorine-based dry etch, see the file File:DryEtchTestsCSAR.pdf. It seems the chlorine etch forms particles of chlorinated CSAR on the surface, and these particles remains on the surface after resist removal with AR-600-71. The C4F8/SF6 etch also forms particles on the surface, but much smaller than those formed in the chlorine etch. It seems these particles are removed after 3 minutes in AR-600-71.
How to mount chips in dry etch tools
All etch rates presented here are measured on chips (i.e. diced 4" wafers) crystal bonded to a carrier. The carrier is either a blank Si wafer, a Si wafer spin coated with resist or a Si wafer coated with ALD grown Al2O3.
Etch Tests of CSAR, recipe 'nano1.42', DRIE PEGASUS, A-1. CSAR thickness measured on Ellipsometer VASE at 70 degrees
Sample
CSAR Etch rate nm/min
Full 4" Si wafer with non-patterned ~180 nm CSAR
~56.5 (based on 2 runs)
Full 4" Si wafer with non-patterned ~240 nm CSAR, postbaked 60 sec @ 130 degC
~56.5 (based on 2 runs)
1/4 4" Si wafer with non-patterned ~125 nm CSAR, not crystal bonded to Si carrier
~83.3 (based on 3 runs)
1/4 4" Si wafer with non-patterned ~125 CSAR, crystal bonded to 4" Si carrier
~54 (based on 1 run)
Etch rates and profile inspection
Continous Etches
Recipe nano1.42 on Deep Reactive Ion Etch PEGASUS A-1
Recipe
Gasses
C4F8 75 sccm, SF6 38 sccm
Profiles of lines exposed at 300 µC/cm2, etched 2:30 minutes (150s) with recipe 'nano1.42'