| | | Simple e-beam pattern in this resist has been tested, the results showed on this page. If you have questions to the process or wish to use this e-beam resist, please contact [mailto:lithography@nanolab.dtu.dk lithography] at DTU Nanolab. |
| {|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" width="90%"
| |
| |-
| |
| | |
| |-
| |
| |-style="background:silver; color:black"
| |
| |'''Resist'''
| |
| |'''Polarity'''
| |
| |'''Manufacturer'''
| |
| |'''Comments'''
| |
| |'''Technical reports'''
| |
| |'''Spinner'''
| |
| |'''Developer'''
| |
| |'''Rinse'''
| |
| |'''Remover'''
| |
| |'''Process flows (in docx-format)'''
| |
| | |
| |-
| |
| | |
| |-
| |
| |-style="background:WhiteSmoke; color:black"
| |
| |'''[[Specific_Process_Knowledge/Lithography/CSAR|CSAR]]'''
| |
| |Positive
| |
| |[http://www.allresist.com AllResist]
| |
| |Standard positive resist, very similar to ZEP520.
| |
| |[[media:Allresist_CSAR62_English.pdf|Allresist_CSAR62_English.pdf]],, [[media:CSAR_62_Abstract_Allresist.pdf|CSAR_62_Abstract_Allresist.pdf]]
| |
| |[[Specific_Process_Knowledge/Lithography/Coaters#Manual Spinner 1|Manual Spinner 1 (Laurell)]], [[Specific_Process_Knowledge/Lithography/Coaters#Spin_coater:_Manual_Labspin|Spin Coater Labspin]]
| |
| |XAR-600-546, XAR-600-548, N50, MIBK:IPA
| |
| |IPA
| |
| |AR-600-71, 1165 Remover
| |
| |[[media:Process_Flow_CSAR.docx|Process_Flow_CSAR.docx]]
| |
| |}
| |
| | |
| | |
| Simple e-beam pattern in this resist has been tested, the results showed on this page. If you have questions to the process or wish to use this e-beam resist, please contact Tine Greibe at tigre@danchip.dtu.dk. | |
| | |
| | |
| == Process Flow ==
| |
| Test of Chemically Semi-Amplified Resist (CSAR); a positive e-beam resist from AllResist (AR-P 6200-2).
| |
| | |
| {|border="1" cellspacing="0" cellpadding="3" style="text-align:left;" style="width: 60%;"
| |
| |-
| |
| | |
| |-
| |
| |-style="background:Black; color:White"
| |
| !Equipment
| |
| !Process Parameters
| |
| !Comments
| |
| |-
| |
| | |
| |-
| |
| |-style="background:WhiteSmoke; color:black; text-align:center"
| |
| !colspan="4"|Pretreatment
| |
| |-
| |
| | |
| | |
| |-
| |
| |-style="background:LightGrey; color:black"
| |
| |4" Si wafers
| |
| |No Pretreatment
| |
| |
| |
| |-
| |
| | |
| |-
| |
| |-style="background:WhiteSmoke; color:black; text-align:center"
| |
| !colspan="4"|Spin Coat
| |
| |-
| |
| | |
| | |
| |-
| |
| |-style="background:LightGrey; color:black"
| |
| |Spin Coater Manual, LabSpin, A-5
| |
| |AR-P 6200/2 AllResist E-beam resist
| |
| 60 sec at various spin speed.
| |
| Acceleration 4000 s-2,
| |
| softbake 1 - 5 min at 150 deg Celcius
| |
| |Disposal pipette used; clean by N2-gun before use. Use approximately 1.5 ml per 4" wafer, never use a pipette twice. Softbake is not a crucial step, see e-mail correspondence with AllResist [[media:Softbake CSAR.pdf|here]].
| |
| |-
| |
| | |
| |-
| |
| |-style="background:WhiteSmoke; color:black; text-align:center"
| |
| !colspan="4"|Characterization
| |
| |-
| |
| | |
| |-
| |
| |-style="background:LightGrey; color:black"
| |
| |Ellipsometer VASE B-1
| |
| |9 points measured on 100 mm wafer
| |
| |ZEP program used; measured at 70 deg only
| |
| |-
| |
| | |
| |-
| |
| |-style="background:WhiteSmoke; color:black; text-align:center"
| |
| !colspan="4"|E-beam Exposure
| |
| |-
| |
| | |
| | |
| |-
| |
| |-style="background:LightGrey; color:black"
| |
| |JEOL 9500 E-beam writer, E-1
| |
| |Dosepattern 15nm - 100nm,
| |
| dose 120-350 muC/cm2
| |
| |Virtual chip mark height detection (CHIPAL V1) used in corner of every dose array
| |
| |-
| |
| | |
| |-
| |
| |-style="background:WhiteSmoke; color:black; text-align:center"
| |
| !colspan="4"|Development
| |
| |-
| |
| | |
| |-
| |
| |-style="background:LightGrey; color:black"
| |
| |Fumehood, D-3
| |
| |60 sec in X AR 600-546,
| |
| 60 sec rinse in IPA,
| |
| N2 Blow dry
| |
| |Gentle agitation while developing. After developing, wafer is immersed in beaker with IPA, subsequently blow dried with N2 gun.
| |
| |-
| |
| | |
| |-
| |
| |-style="background:WhiteSmoke; color:black; text-align:center"
| |
| !colspan="4"|Characterization
| |
| |-
| |
| | |
| |-
| |
| |-style="background:LightGrey; color:black"
| |
| |Zeiss SEM Supra 60VP, D-3
| |
| |2-3 kV, shortest working distance possible, chip mounted with Al tape
| |
| |For dosepattern SEM inspection: the wafers are diced into smaller pieces and sputter coated with Pt at DTU CEN before SEM inspection; please contact [mailto:ramona.mateiu@cen.dtu.dk Ramona Valentina Mateiu] for further information.
| |
| |-
| |
| | |
| |}
| |
|
| |
|
| == Spin Curves == | | == Spin Curves == |
|
| |
|
|
| |
|
| [[File:SpinCurveCSAR.jpg|right|600px]]
| | The thickness is measured on VASE Ellipsometer using a simple Cauchy model for a transparent polymer on Si. The measurements are performed at one incidence angle (70 degrees) only. 9 points on each 4" wafer has been measured; the standard deviation thus representing the homogeinity of the film on the 4" wafers. |
|
| |
|
| The thickness is measured on VASE Ellipsometer using a simple Cauchy model for a transparent polymer on Si. The measurements are performed at one incidence angle (70 degrees) only. 9 points on each 4" wafer has been measured; the standard deviation thus representing the homogeinity of the film on the 4" wafers.
| | Around 2 ml of resist per wafer has been used when fabricating these curves. If you use less than 2 ml, the thickness of the final resist might be smaller than reported here. |
|
| |
|
| Please be aware that I have experienced a somewhat large thickness deviation (5-8 %) depending on the amount of resist applied to the wafer before spin coating.
| |
|
| |
|
| <span style="color:#696969">'''Dosepattern has been e-beam exposured and SEM inspected on those wafers marked by silver gray.'''</span>
| | [[File:CSAR_09.png|right|600px]] |
| | [[File:CSAR_18.png|right|600px]] |
|
| |
|
|
| |
|
| Line 150: |
Line 19: |
|
| |
|
| |- | | |- |
| |-style="background:Black; color:White" | | |-style="background:#00308F; color:White" |
| !colspan="7"|AllResist AR-P 6200 (> 2ml per 4" wafer) spinning on Spin Coater: Manual LabSpin A-5, TIGRE, 09-04-2014. Softbake 5 min @ 150 degC. | | !colspan="7"|AllResist AR-P 6200.09 (> 2ml per 4" wafer) spinning on Spin Coater: Manual LabSpin A-5, TIGRE, 09-04-2014. Softbake 5 min @ 150 degC. |
| |- | | |- |
|
| |
|
| |- | | |- |
| |-style="background:WhiteSmoke; color:black" | | |-style="background:silver; color:black" |
| !Spin Speed [rpm] | | !Spin Speed [rpm] |
| !Acceleration [1/s2] | | !Acceleration [1/s2] |
| !Thickness [nm] | | !Thickness [nm] |
| !St Dev
| |
| |- | | |- |
|
| |
|
| Line 166: |
Line 34: |
| |2000 | | |2000 |
| |4000 | | |4000 |
| |225.98 | | |226 |
| |0.97
| |
| |- | | |- |
|
| |
|
| Line 174: |
Line 41: |
| |3000 | | |3000 |
| |4000 | | |4000 |
| |194.00 | | |194 |
| |0.6
| |
| |- | | |- |
|
| |
|
| Line 182: |
Line 48: |
| |4000 | | |4000 |
| |4000 | | |4000 |
| |169.57 | | |170 |
| |0.32
| |
| |- | | |- |
|
| |
|
| Line 190: |
Line 55: |
| |5000 | | |5000 |
| |4000 | | |4000 |
| |151.47 | | |151 |
| |0.26
| |
| |- | | |- |
|
| |
|
| |- | | |- |
| |-style="background:Silver; color:black" | | |-style="background:WhiteSmoke; color:black" |
| |6000 | | |6000 |
| |4000 | | |4000 |
| |142.38 | | |142 |
| |0.41
| |
| |- | | |- |
|
| |
|
| Line 206: |
Line 69: |
| |7000 | | |7000 |
| |4000 | | |4000 |
| |126.59 | | |127 |
| |0.36
| |
| |- | | |- |
|
| |
|
| Line 218: |
Line 80: |
|
| |
|
| |- | | |- |
| |-style="background:green; color:White" | | |-style="background:red; color:White" |
| !colspan="7"|AllResist CSAR (< 2ml per 4" wafer) on Spin Coater: Manual LabSpin A-5, TIGRE, 16-06-2014. Softbake 2 min @ 150 degC. | | !colspan="7"|AllResist CSAR 6200.09 1:1 in anisole (< 2ml per 4" wafer), Spin Coater: Manual LabSpin A-5, TIGRE, 16-06-2014. Softbake 2 min @ 150 degC. |
| |- | | |- |
|
| |
|
| Line 227: |
Line 89: |
| !Acceleration [1/s2] | | !Acceleration [1/s2] |
| !Thickness [nm] | | !Thickness [nm] |
| !St Dev
| | |- |
| | |
| | |- |
| | |-style="background:WhiteSmoke; color:black" |
| | |2000 |
| | |4000 |
| | |84 |
| |- | | |- |
|
| |
|
| Line 234: |
Line 102: |
| |3000 | | |3000 |
| |4000 | | |4000 |
| |201.61 | | |67 |
| |1.20
| |
| |- | | |- |
|
| |
|
| Line 242: |
Line 109: |
| |4000 | | |4000 |
| |4000 | | |4000 |
| |173.89 | | |59 |
| |0.64
| |
| |- | | |- |
|
| |
|
| Line 250: |
Line 116: |
| |5000 | | |5000 |
| |4000 | | |4000 |
| |155.91 | | |53 |
| |0.65 | | |- |
| | |
| | |- |
| | |-style="background:WhiteSmoke; color:black" |
| | |6000 |
| | |4000 |
| | |49 |
| |- | | |- |
|
| |
|
| Line 262: |
Line 134: |
|
| |
|
| |- | | |- |
| |-style="background:red; color:White" | | |-style="background:green; color:White" |
| !colspan="7"|AllResist CSAR 1:1 in anisole (< 2ml per 4" wafer), Spin Coater: Manual LabSpin A-5, TIGRE, 16-06-2014. Softbake 2 min @ 150 degC. | | !colspan="7"|AllResist CSAR 6200.18 (< 2ml per 4" wafer), Spin Coater: Manual Standard Resists, E-5, TIGRE, 15-06-2016. Softbake 2 min @ 180 degC. |
| |- | | |- |
|
| |
|
| Line 271: |
Line 143: |
| !Acceleration [1/s2] | | !Acceleration [1/s2] |
| !Thickness [nm] | | !Thickness [nm] |
| !St Dev
| |
| |- | | |- |
|
| |
|
| Line 277: |
Line 148: |
| |-style="background:WhiteSmoke; color:black" | | |-style="background:WhiteSmoke; color:black" |
| |2000 | | |2000 |
| |4000 | | |2000 |
| |83.48 | | |1003 |
| |0.49
| |
| |- | | |- |
|
| |
|
| Line 285: |
Line 155: |
| |-style="background:WhiteSmoke; color:black" | | |-style="background:WhiteSmoke; color:black" |
| |3000 | | |3000 |
| |4000 | | |2000 |
| |67.12 | | |809 |
| |0.41
| |
| |- | | |- |
|
| |
|
| Line 293: |
Line 162: |
| |-style="background:WhiteSmoke; color:black" | | |-style="background:WhiteSmoke; color:black" |
| |4000 | | |4000 |
| |4000 | | |2000 |
| |58.64 | | |721 |
| |0.44
| |
| |- | | |- |
|
| |
|
| |- | | |- |
| |-style="background:Silver; color:black" | | |-style="background:WhiteSmoke; color:black" |
| |5000 | | |5000 |
| |4000 | | |2000 |
| |53.13 | | |639 |
| |0.39
| |
| |- | | |- |
|
| |
|
| Line 309: |
Line 176: |
| |-style="background:WhiteSmoke; color:black" | | |-style="background:WhiteSmoke; color:black" |
| |6000 | | |6000 |
| |4000 | | |2000 |
| |48.76 | | |586 |
| |0.38
| |
| |- | | |- |
|
| |
|
| | |- |
| | |-style="background:WhiteSmoke; color:black" |
| | |7000 |
| | |2000 |
| | |549 |
| | |- |
| |} | | |} |
|
| |
|
| == Contrast Curves ==
| |
|
| |
|
| 100 nm lines in ~145 nm thick CSAR has been developed with AR-600-546 (standard CSAR developer) with and without agitation at room temperature and at 5 degrees Celsius. Furthermore, same pattern ahs been developed with N50 (standard developer for ZEP520A). | | == Contrast Curve == |
| | |
| | === CSAR 6200.09 === |
| | |
| | 100 nm lines in both ~70 nm and ~188 nm thick CSAR has been developed with AR-600-546 (standard CSAR developer) at room temperature to provide the following contrast curves. |
|
| |
|
| {|border="1" cellspacing="0" cellpadding="3" style="text-align:left;" style="width: 95%" | | {|border="1" cellspacing="0" cellpadding="3" style="text-align:left;" style="width: 95%" |
| Line 325: |
Line 200: |
| |- | | |- |
| |-style="background:Black; color:White" | | |-style="background:Black; color:White" |
| !colspan="5"|wafer 9.19 Contrast Curve, Processed by TIGRE, Dec-Jan 2014-2015 | | !colspan="5"|CSAR Contrast Curve, Processed by TIGRE, FEB-MARCH 2016 |
| |- | | |- |
|
| |
|
| Line 339: |
Line 214: |
| |- | | |- |
| |-style="background:WhiteSmoke; color:black" | | |-style="background:WhiteSmoke; color:black" |
| |CSAR AR-P6200 AllResist | | |CSAR AR-P6200.09 AllResist, CSAR AR-P6200.09 diluted 1:1 in Anisole |
| |19-12-2014, LabSpin A-1, 4000 rpm, 60s, softbaked 60s @ 150degC | | |08-02-2016, LabSpin E-5, 4000 rpm, 60s, softbaked 60s @ 205 degC |
| |19-12-2014, JBX9500 E-2, 2nA aperture 5, doses 60-600 µC/cm2, 100 nm lines with 300 nm spaces | | |09-02-2016, JBX9500 E-2, 2nA aperture 5, doses 40-600 µC/cm2, 100 nm lines and 300 nm spaces |
| |22-12-2014, 05-01-2015, Fumehood D-2, misc developers, rinsed in IPA 60s. The cold development was performed with developer stored in refrigerator (Cx1), exact temperature was not measured. | | |11-02-2016, Fumehood D-2, AR-600-546, rinsed in IPA 60s. |
| |23-12-2014, 05-01-2015, Zeiss Supra 60VP, 10kV, Inlens detector, stage at - 4-5 degrees. Samples '''not''' coated before inspection. | | |02-03-2016 AFM Icon, F-2, ScanAsyst in Air |
| |- | | |- |
|
| |
|
| |} | | |} |
|
| |
|
| [[File:ContrastCurvesCSAR.png|500px]]
| | {| style="border: none; border-spacing: 0; margin: 1em auto; text-align: center;" |
| [[File:w919sa-d.png|500px]]
| |
| | |
| == Dosetests ==
| |
| | |
| | |
| | |
| So far (September 2014) three wafers with CSAR have been e-beam exposed with dosetests and inspected in SEM. Thickness of resist, e-beam dose and development time has been changed somewhat from wafer to wafer:
| |
| | |
| | |
| {|border="1" cellspacing="0" cellpadding="3" style="text-align:left;" style="width: 60%;" | |
| |-
| |
| | |
| |-
| |
| |-style="background:Black; text-align:left; color:White"
| |
| !rowspan="2"|Process
| |
| !rowspan="2"|Equipment
| |
| !colspan="3"|Parameters
| |
| |-
| |
| | |
| |-
| |
| |-style="background:Black; text-align:left; color:White"
| |
| !6.13
| |
| !4.09
| |
| !3.05
| |
| |-
| |
| | |
| | |
| |-
| |
| |-style="background:WhiteSmoke; color:black"
| |
| |Resist
| |
| |Fumehood D-3
| |
| |'''Resist:''' AR-P 6200/2 diluted 1:1 in anisole (Bottled opened 16-06-2014 TIGRE)
| |
| |'''Resist:''' AR-P 6200/2 diluted 1:1 in anisole (Bottled opened 16-06-2014 TIGRE)
| |
| |'''Resist:''' AR-P 6200/2
| |
| |-
| |
| |-style="background:WhiteSmoke; color:black"
| |
| |Spin Coat
| |
| |Spin Coater LabSpin A-5
| |
| |'''Spin:''' 1 min @ 6000 rpm,<br /> '''softbake:''' 1 min @ 150 degC, <br />'''thickness:''' ~50nm <br />(27-08-2014 TIGRE)
| |
| |'''Spin:''' 1 min @ 5000 rpm,<br /> '''softbake:''' 2 min @ 150 degC, <br />'''thickness:''' ~53nm <br />(16-06-2014 TIGRE)
| |
| |'''Spin:''' 1 min @ 6000 rpm,<br /> '''softbake:''' 5 min @ 150 degC, <br />'''thickness:''' ~143nm <br />(09-04-2014 TIGRE)
| |
| |-
| |
| |-
| |
| |-style="background:WhiteSmoke; color:black"
| |
| |E-beam exposure
| |
| |JEOL 9500 E-2
| |
| |'''Condition file:''' 0.2nA_ap5,<br /> '''doses:''' 180-420 muC/cm2,<br /> '''Shot pitch:''' 7-27 nm,<br /> '''PEC:''' no <br />(27-08-2014 TIGRE)
| |
| |'''Condition file:''' 0.2nA_ap5,<br /> '''doses:''' 207-242 muC/cm2,<br /> '''Shot pitch:''' 5 nm,<br /> '''PEC:''' no <br />(02-07-2014 TIGRE)
| |
| |'''Condition file:''' 2nA_ap5,<br /> '''doses:''' 207-242 muC/cm2,<br /> '''Shot pitch:''' 5 nm,<br /> '''PEC:''' no <br />(10-04-2014 TIGRE)
| |
| |-
| |
| |-
| |
| |-style="background:WhiteSmoke; color:black"
| |
| |Develop
| |
| |Fumehood D-3
| |
| |'''Developer:''' SX-AR 600-54/6,<br /> '''time:''' 30 sec,<br /> '''Rinse:''' 30 sec in IPA<br /> (28-08-2014 TIGRE)
| |
| |'''Developer:''' SX-AR 600-54/6,<br /> '''time:''' 60 sec,<br /> '''Rinse:''' 30 sec in IPA<br /> (08-07-2014 TIGRE)
| |
| |'''Developer:''' SX-AR 600-54/6,<br /> '''time:''' 60 sec,<br /> '''Rinse:''' 60 sec in IPA<br /> (April/May-2014 TIGRE)
| |
| |-
| |
| |-
| |
| |-style="background:WhiteSmoke; color:black"
| |
| |Sputter Coat
| |
| |Cressington 208HR, DTU CEN, please contact [mailto:ramona.mateiu@cen.dtu.dk Ramona Valentina Mateiu] for information
| |
| |3-5 nm Pt, sputtering, (29-08-2014 TIGRE)
| |
| |3-5 nm Pt, sputtering (09-07-2014 TIGRE)
| |
| |3-5 nm Pt, sputtering (22-05-2014 TIGRE)
| |
| |-
| |
| |-
| |
| |-style="background:WhiteSmoke; color:black"
| |
| |Characterization
| |
| |Zeiss SEM Supra 60VP, D-3
| |
| |'''Acc voltage:''' 3 kV,<br /> '''WD:''' < 4mm, <br />conducting tape close to pattern (29-08-2014 TIGRE)
| |
| |'''Acc voltage:''' 3 kV,<br /> '''WD:''' < 4mm, <br />conducting tape close to pattern (09-07-2014 TIGRE)
| |
| |'''Acc voltage:''' 2 kV,<br /> '''WD:''' < 4mm, <br />conducting tape close to pattern (06-06-2014 TIGRE)
| |
| |- | | |- |
| | | [[image:ContrastCurvesCSAR_March2016_log.png|600px]] |
| | |- |
| | | colspan="1" style="text-align:center;| |
| | AR-P 6200 contrast curves. |
| |} | | |} |
|
| |
|
| | ==Dose to size== |
| | Small features need a comparatively higher dose then big features and hence it can be useful to map out the dose and size dependency. Below is a set of cross sectional images of 100, 50 and 20 nm lines written 500, 250 and 180 nm resist at doses from 200 to 600 µC/cm<sup>2</sup>. |
|
| |
|
| | | {| style="border: none; border-spacing: 0; margin: 1em auto; text-align: center;" |
| {| class="wikitable collapsible collapsed" style="border: 5px solid black;" style="width: 90%;" align="center" | |
| !colspan="8"| SEM inspection of wafer 6.13, 100 nm exposed pattern, shot pitch 7 nm
| |
| |- | | |- |
| | | [[image:thope240214_lines_100_06.png|1200px]] |
| | |- |
| | | [[image:thope240214_lines_50_11.png|1200px]] |
| | |- |
| | | [[image:thope240214_lines_20_13.png|1200px]] |
| |- | | |- |
| ! 300 [muC/cm2]
| | | colspan="1" style="text-align:center;| |
| | [[File:6_13_100nm_300_shot14.png|230px]] | | Cross section SEM images of 500 nm AR-P 6200.09 exposed at 200-600 µC/cm<sup>2</sup>. Top image is 100 nm lines, center image is 50 nm lines, bottom image is 20 nm lines. Au coated for SEM imaging. |
| | [[File:6_13_100nm_300_shot14_Lines.png|230px]]
| |
| | [[File:6_13_100nm_300_shot14_Holes.png|230px]]
| |
| | [[File:6_13_100nm_300_shot14_Holes2.png|230px]]
| |
| | [[File:6_13_100nm_300_shot14_Pillars.png|230px]]
| |
| | [[File:6_13_100nm_300_shot14_Test.png|230px]]
| |
| ! ACHK NOT READY
| |
| |-
| |
| |} | | |} |
|
| |
|
| {| class="wikitable collapsible collapsed" style="border: 5px solid black;" style="width: 90%;" align="center" | | {| style="border: none; border-spacing: 0; margin: 1em auto; text-align: center;" |
| !colspan="7"| SEM inspection of wafer 6.13, 50 nm exposed pattern, shot pitch 7 nm
| |
| |- | | |- |
| |-
| | | [[image:thope240214_lines250_100nm.png|1200px]] |
| ! 270 [muC/cm2]
| |
| | [[File:6_13_50nm_270_shot14.png|230px]]
| |
| | [[File:6_13_50nm_270_shot14_Lines.png|230px]]
| |
| | [[File:6_13_50nm_270_shot14_Holes.png|230px]]
| |
| | [[File:6_13_50nm_270_shot14_Pillars.png|230px]]
| |
| | [[File:6_13_50nm_270_shot14_Holes2.png|230px]] | |
| ! ACHK NOT READY
| |
| |- | | |- |
| | | | [[image:thope240214_lines250_50nm.png|1200px]] |
| |- | | |- |
| ! 300 [muC/cm2]
| | | [[image:thope240214_lines250_20nm.png|1200px]] |
| | [[File:6_13_50nm_300_shot14.png|230px]]
| |
| | [[File:6_13_50nm_300_shot14_Lines.png|230px]]
| |
| | [[File:6_13_50nm_300_shot14_Holes.png|230px]]
| |
| | [[File:6_13_50nm_300_shot14_Pillars.png|230px]]
| |
| | [[File:6_13_50nm_300_shot14_Holes2.png|230px]] | |
| ! ACHK NOT READY
| |
| |- | | |- |
| | | colspan="1" style="text-align:center;| |
| | Cross section SEM images of 250 nm AR-P 6200.09 exposed at 200-600 µC/cm<sup>2</sup>. Top image is 100 nm lines, center image is 50 nm lines, bottom image is 20 nm lines. Au coated for SEM imaging. |
| |} | | |} |
|
| |
|
| {| class="wikitable collapsible collapsed" style="border: 5px solid black;" style="width: 90%;" align="center" | | {| style="border: none; border-spacing: 0; margin: 1em auto; text-align: center;" |
| !colspan="6"| SEM inspection of wafer 6.13, 30 nm exposed pattern, shot pitch 7 nm
| |
| |- | | |- |
| |-
| | | [[image:thope240214_lines180_100_29.png|1200px]] |
| ! 240 [muC/cm2]
| |
| | [[File:6_13_30nm_240_shot14.png|230px]] | |
| | [[File:6_13_30nm_240_shot14_Lines.png|230px]]
| |
| |
| |
| |
| |
| | ACHK NOT READY
| |
| |- | | |- |
| | | [[image:thope240214_lines180_50_31.png|1200px]] |
| |- | | |- |
| ! 270 [muC/cm2]
| | | [[image:thope240214_lines180_20_33.png|1200px]] |
| | [[File:6_13_30nm_270_shot14.png|230px]]
| |
| | [[File:6_13_30nm_270_shot14_Lines.png|230px]]
| |
| | [[File:6_13_30nm_270_shot14_Holes.png|230px]] | |
| | [[File:6_13_30nm_270_shot14_Pillars.png|230px]]
| |
| | ACHK NOT READY
| |
| |- | | |- |
| |- | | | colspan="1" style="text-align:center;| |
| ! 300 [muC/cm2]
| | Cross section SEM images of 180 nm AR-P 6200.09 exposed at 200-600 µC/cm<sup>2</sup>. Top image is 100 nm lines, center image is 50 nm lines, bottom image is 20 nm lines. Au coated for SEM imaging. |
| | [[File:6_13_30nm_300_shot14.png|230px]]
| |
| | [[File:6_13_30nm_300_shot14_Lines.png|230px]]
| |
| | [[File:6_13_30nm_300_shot14_Holes.png|230px]]
| |
| | [[File:6_13_30nm_300_shot14_Pillars.png|230px]]
| |
| | ACHK NOT READY
| |
| |-
| |
| |} | | |} |
|
| |
|
| {| class="wikitable collapsible collapsed" style="border: 5px solid black;" style="width: 90%;" align="center"
| | === CSAR 6200.18 === |
| !colspan="4"| SEM inspection of wafer 6.13, 20 nm exposed pattern, shot pitch 7 nm
| |
|
| |
|
| |-
| | 100 nm lines in ~900 nm thick CSAR has been developed with AR-600-546 (standard CSAR developer) at room temperature. |
| |-
| |
| ! 270 [muC/cm2]
| |
| | [[File:6_13_20nm_270_shot14.png|230px]]
| |
| | [[File:6_13_20nm_270_shot14_Lines.png|230px]]
| |
| | ACHK NOT READY
| |
| |-
| |
| |-
| |
| ! 300 [muC/cm2]
| |
| | [[File:6_13_20nm_300_shot14.png|230px]]
| |
| | [[File:6_13_20nm_300_shot14_Lines.png|230px]]
| |
| | ACHK NOT READY
| |
| |-
| |
| |}
| |
|
| |
|
| | [[File:CSAR 6200.18 developed with AR600546.png|right|400px]] |
|
| |
|
| | | {|border="1" cellspacing="0" cellpadding="3" style="text-align:right;" style="width: 60%" |
| {| class="wikitable collapsible collapsed" style="border: 5px solid black;" style="width: 90%;" align="center" | |
| !colspan="6"| SEM inspection of wafer 4.09, 50 nm exposed pattern, shot pitch 5 nm
| |
| |- | | |- |
| ! 230 [muC/cm2]
| |
| | [[File:53nmCSAR50nmOverviewBasedose.png|250px]]
| |
| | [[File:53nmCSAR50nmLinesBasedose.png|250px]]
| |
| | [[File:53nmCSAR50nmHolesBasedose.png|250px]]
| |
| | [[File:53nmCSAR50nmPillarsBasedose.png|250px]]
| |
| | [[File:53nmCSAR50nmTestBasedose.png|250px]]
| |
| |}
| |
|
| |
|
| {| class="wikitable collapsible collapsed" style="border: 5px solid black;" style="width: 90%;" align="center"
| |
| !colspan="4"| SEM inspection of wafer 4.09, 30 nm exposed pattern, shot pitch 5 nm
| |
| |- | | |- |
| |- | | |-style="background:Black; color:White" |
| ! 219 [muC/cm2] | | !colspan="5"|CSAR Contrast Curve, Processed by TIGRE, JUNE 2016 |
| | [[File:53nmCSAR30nmOverviewBasedose-5%.png|250px]]
| |
| | [[File:53nmCSAR30nmLinesBasedose-5%.png|250px]]
| |
| | [[File:30nmShot10.png|250px]]
| |
| |- | | |- |
| |-
| | |
| ! 230 [muC/cm2]
| |
| | [[File:53nmCSAR30nmOverviewBasedose.png|250px]]
| |
| | [[File:53nmCSAR30nmLinesBasedose.png|250px]]
| |
| |
| |
| |- | | |- |
| |- | | |-style="background:WhiteSmoke; color:black" |
| ! 242 [muC/cm2] | | !Resist |
| | [[File:53nmCSAR30nmOverviewBasedose+5%.png|250px]]
| | !Spin Coat |
| | [[File:53nmCSAR30nmLinesBasedose+5%.png|250px]]
| | !E-beam exposure |
| |
| | !Development |
| | !Characterisation |
| |- | | |- |
| |}
| |
|
| |
|
| {| class="wikitable collapsible collapsed" style="border: 5px solid black;" style="width: 90%;" align="center"
| |
| !colspan="4"| SEM inspection of wafer 4.09, 20 nm exposed pattern, shot pitch 5 nm
| |
| |- | | |- |
| |- | | |-style="background:WhiteSmoke; color:black" |
| ! 230 [muC/cm2]
| | |CSAR AR-P6200.18 AllResist |
| | [[File:53nmCSAR20nmOverviewBasedose.png|220px]]
| | |15-06-2016, LabSpin E-5, 2000 rpm, 60s, softbaked 60s @ 205 degC |
| | [[File:53nmCSAR20nmLinesBasedose.png|220px]]
| | |15-06-2016, JBX9500 E-2, 2nA aperture 5, doses 40-600 µC/cm2, 100 nm lines and 300 nm spaces |
| | [[File:20nmShot10.png|220px]] | | |16-06-2016, Fumehood E-4, AR-600-546, 30s/60s/90s, rinsed in IPA 60s. |
| |- | | |JUNE/JULY 2016 SEM Supra 2, 10 keV |
| |- | |
| ! 242 [muC/cm2]
| |
| | [[File:53nmCSAR20nmOverviewBasedose+5%.png|220px]]
| |
| | [[File:53nmCSAR20nmLines2Basedose+5%.png|220px]]
| |
| |
| |
| |- | |
| |-
| |
| ! 253 [muC/cm2]
| |
| | [[File:53nmCSAR20nmOverviewBasedose+10%.png|220px]]
| |
| | [[File:53nmCSAR20nmLinesBasedose+10%.png|220px]] | |
| |
| |
| |- | | |- |
| | |
| |} | | |} |
|
| |
|
| {| class="wikitable collapsible collapsed" style="border: 5px solid black;" style="width: 90%;" align="center"
| | <br clear="all"/> |
| !colspan="4"| SEM inspection of wafer 4.09, 15 nm exposed pattern, shot pitch 5 nm
| | |
| |-
| | |
| |-
| | === Dark Erosion === |
| ! 253 [muC/cm2]
| | |
| | [[File:53nmCSAR15nmOverviewBasedose+10%.png|250px]]
| | Dark erosion has been measured on a un-exposed 4" wafer spin coated with CSAR 6200.18 to a thickness of approximately 549 nm. The resist thickness has been measured by VASE Ellipsometer before development, and after 3 minutes, 13 minutes, and 30 minutes of development in AR 600 546. |
| | [[File:53nmCSAR15nmLinesBasedose+10%.png|250px]] | | |
| |[[File:15nmShot10.png|250px]]
| | The graphs shows the measured thicknesses; the errorbars represents the standard deviations from the ellipsometric measurements. The average etch rate of CSAR is ~0.1 nm/min. |
| |-
| | |
| |-
| | [[File:dark erosion.png|right|400px]] |
| ! 276 [muC/cm2]
| | |
| | [[File:53nmCSAR15nmOverviewBasedose+20%.png|250px]]
| | |
| | [[File:53nmCSAR15nmLinesBasedose+20%.png|250px]]
| | |
| |
| | <br clear="all" /> |
| |-
| | |
| |}
| | == Development == |
| | |
| | Many resists can be developed in different developers, CSAR can be developed in: AR 600-546, AR 600-548, ZED N-50 and mix of MIBK and IPA among others. |
|
| |
|
| | CSAR and ZEP520A are in principle the same chemical, however the pretreatment (filtration and temperature control) can differ. |
|
| |
|
| {| class="wikitable collapsible collapsed" style="border: 5px solid black;" style="width: 90%;" align="center"
| | Some users have reported residues and residual layers when using ZED N-50 on CSAR and vice verca, hence we recommend to use AR 600-546 or AR 600-548 (3 times stronger) to develop CSAR and not ZED N-50. |
| !colspan="4"| SEM inspection of wafer 3.05, 50 nm exposed pattern, shot pitch 5 nm
| |
| |-
| |
| |-
| |
| ! 207 [muC/cm2]
| |
| | [[File:CSAR50nmoverview-10%.png|270px]]
| |
| | [[File:CSAR50nmlines-10%.png|270px]]
| |
| |NO ACHK READY
| |
| |-
| |
| |-
| |
| ! 219 [muC/cm2]
| |
| | [[File:CSAR50nmoverview-5%.png|270px]]
| |
| | [[File:CSAR50nmlines-5%.png|270px]]
| |
| |
| |
| |-
| |
| |-
| |
| ! 230 [muC/cm2]
| |
| | [[File:CSAR50nmoverview.png|270px]]
| |
| | [[File:CSAR50nmlines.png|270px]]
| |
| |
| |
| |-
| |
| |-
| |
| ! 242 [muC/cm2]
| |
| | [[File:CSAR50nmoverview+5%.png|270px]]
| |
| | [[File:CSAR50nmlines+5%.png|270px]]
| |
| |
| |
| |-
| |
| |}
| |
|
| |
|
| {| class="wikitable collapsible collapsed" style="border: 5px solid black;" style="width: 90%;" align="center"
| | When this is said some users still observe residues when using AR 600-546, the producer "'''All resist GMBH'''" have recommended to use 3-5s, dip in pure MIBK to remove residues. |
| !colspan="4"| SEM inspection of wafer 3.05, 30 nm exposed pattern, shot pitch 5 nm
| | |
| |-
| | AR 600 546 will dissolve different plastic materials, hence never use it on PS compounds. |
| |-
| |
| ! 207 [muC/cm2]
| |
| | [[File:CSAR30nmoverview-10%.png|270px]]
| |
| | [[File:CSAR30nmlines-10%.png|270px]]
| |
| |NO ACHK READY
| |
| |-
| |
| |-
| |
| ! 219 [muC/cm2]
| |
| | [[File:CSAR30nmoverview-5%.png|270px]]
| |
| | [[File:CSAR30nmlines-5%.png|270px]]
| |
| |
| |
| |-
| |
| |-
| |
| ! 230 [muC/cm2]
| |
| | [[File:CSAR30nmoverview.png|270px]]
| |
| | [[File:CSAR30nmlines.png|270px]]
| |
| |
| |
| |-
| |
| |-
| |
| ! 242 [muC/cm2]
| |
| | [[File:CSAR30nmoverview+5%.png|270px]]
| |
| | [[File:CSAR30nmlines+5%.png|270px]]
| |
| |
| |
| |-
| |
| |}
| |
|
| |
|
| {| class="wikitable collapsible collapsed" style="border: 5px solid black;" style="width: 90%;" align="center"
| | <br clear="all"/> |
| !colspan="4"| SEM inspection of wafer 3.05, 20 nm exposed pattern, shot pitch 5 nm
| |
| |-
| |
| |-
| |
| ! 207 [muC/cm2]
| |
| | [[File:CSAR30nmoverview-10%.png|270px]]
| |
| | [[File:CSAR30nmlines-10%.png|270px]]
| |
| |NO ACHK READY
| |
| |-
| |
| |-
| |
| ! 230 [muC/cm2]
| |
| | [[File:CSAR20nmoverview.png|280px]]
| |
| |
| |
| |-
| |
| |-
| |
| ! 242 [muC/cm2]
| |
| | [[File:CSAR20nmoverview+5%.png|280px]]
| |
| |
| |
| |-
| |
| |-
| |
| ! 253 [muC/cm2]
| |
| | [[File:CSAR20nmoverview+10%.png|280px]]
| |
| |
| |
| |-
| |
| |}
| |
|
| |
|
| == Etch Tests == | | == Etch Tests == |
|
| |
|
| The tests presented here are prelimenary results and this page will be updated regularly. I post this as the interest in etch resistance of CSAR is increasing; if you have wafers or chips you would like to have tested, please send me an [[mailto:tigre@danchip.dtu.dk email]].
| | If you have wafers or chips with CSAR you would like to have tested, please send me an [[mailto:tigre@danchip.dtu.dk email]]. |
|
| |
|
| === Chlorine versus flourine-based etches === | | === Chlorine versus flourine-based etches === |
| Line 688: |
Line 347: |
| {|border="1" cellspacing="0" cellpadding="3" style="text-align:left;" style="width: 40%;" | | {|border="1" cellspacing="0" cellpadding="3" style="text-align:left;" style="width: 40%;" |
| |- | | |- |
| |+style="background:Black; color:White" colspan="4"|'''Etch Tests of CSAR, recipe 'nano1.42', DRIE PEGASUS, A-1''' | | |+style="background:Black; color:White" colspan="4"|'''Etch Tests of CSAR, recipe 'nano1.42', DRIE PEGASUS, A-1. CSAR thickness measured on Ellipsometer VASE at 70 degrees''' |
| |-
| |
| |-
| |
| !rowspan="2"|Sample
| |
| !colspan="1"|Etch rate nm/min
| |
| |- | | |- |
| |- | | |- |
| |CSAR (Ellipsometer) | | !rowspan="1"|Sample |
| |- | | !colspan="1"|CSAR Etch rate nm/min |
| |- | | |- |
| |Full 4" Si wafer with non-patterned ~180 nm CSAR | | |Full 4" Si wafer with non-patterned ~180 nm CSAR |
| Line 728: |
Line 383: |
| | Gasses | | | Gasses |
| | C<sub>4</sub>F<sub>8</sub> 75 sccm, SF<sub>6</sub> 38 sccm | | | C<sub>4</sub>F<sub>8</sub> 75 sccm, SF<sub>6</sub> 38 sccm |
| |rowspan="7" | Profiles of lines exposed at 300 µC/cm2 | | |rowspan="7" width="20%" | Profiles of lines exposed at 300 µC/cm2, etched 2:30 minutes (150s) with recipe 'nano1.42' |
| [[File:617817 HD-4_18.png|200px]] [[File:617817 HD-4_11.png|200px]] [[File:617817 HD-4_14.png|200px]] [[File:617817 HD-4_16.png|200px]] | | [[File:617817 HD-4_11.png|200px]] [[File:617817 HD-4_18.png|200px]] |
| | [[File:617817 HD-4_16.png|200px]] [[File:617817 HD-4_14.png|200px]] |
| |- | | |- |
| | Pressure | | | Pressure |
| Line 752: |
Line 408: |
| ! rowspan="2" align="center"| Etch rates | | ! rowspan="2" align="center"| Etch rates |
| | Si | | | Si |
| | 500 nm lines: ~500 nm/min | | | |
| 190 nm lines: ~500 nm/min | | 500 nm lines: ~200 nm/min <br> |
| 102 nm lines: ~490 nm/min | | 190 nm lines: ~200 nm/min <br> |
| 61 nm lines: ~440 nm/min | | 102 nm lines: ~190 nm/min <br> |
| | 61 nm lines: ~170 nm/min |
| |- | | |- |
| |CSAR | | |CSAR |
| | ~55 nm/min | | | ~55 nm/min |
| | |- |
| | |} |
| | |
| | |
| | |
| | {|border="1" cellspacing="0" cellpadding="3" style="text-align:left;" style="width: 80%;" |
| | |- |
| | |+style="background:Black; color:White" colspan="4"|'''Recipe processC on Deep Reactive Ion Etch PEGASUS A-1''' |
| | |- |
| | |- |
| | ! rowspan="4" align="center"| Recipe |
| | | Gasses |
| | | C<sub>4</sub>F<sub>8</sub> 70 sccm, SF<sub>6</sub> 38 sccm |
| | |rowspan="7" width="20%" | Profiles of lines exposed at 300 µC/cm2, etched 60s with recipe 'ProcessC' |
| | [[File:tigre 6.17 0% 3b_ 07.png|200px]] [[File:tigre 6.17 0% 3b_ 16.png|200px]] |
| | [[File:tigre 6.17 0% 3b_ 14.png|200px]] [[File:tigre 6.17 0% 3b_ 11.png|200px]] |
| | |- |
| | | Pressure |
| | | 4 mTorr, |
| | Strike: secs @ mTorr |
| | |
| | |- |
| | | Power |
| | | 450 W Coil Power, 100 W Platen Power |
| | |- |
| | |Platen temperature |
| | | 10°C |
| | |- |
| | |
| | ! rowspan="1" align="center"| Conditions |
| | | Conditioning |
| | | Pre-clean: 10 min oxygen clean |
| | 5 min oxygen clean between runs |
| | |- |
| | ! rowspan="2" align="center"| Etch rates |
| | | Si |
| | | |
| | 500 nm lines: ~300 nm/min <br> |
| | 102 nm lines: ~250 nm/min <br> |
| | |
| | |- |
| | |CSAR |
| | | 158 nm/min |
| | |- |
| | |} |
| | |
| | ==== Bosch Etch ==== |
| | |
| | |
| | {|border="1" cellspacing="0" cellpadding="3" style="text-align:left;" style="width: 80%;" |
| | |- |
| | |+style="background:Black; color:White" colspan="4"|'''Recipe NBoost01 on Deep Reactive Ion Etch PEGASUS A-1''' |
| | |- |
| | |- |
| | ! rowspan="13" align="center" width ="70"| Recipe |
| | | rowspan="4" width ="50"| Deposition step |
| | |Duration |
| | | width ="100" |2.5 s |
| | |rowspan="16" width="20%" | Profiles of lines exposed at 300 µC/cm2, etched 6:00 minutes with recipe 'NBoost01' |
| | [[File:tigre 6.17 -15% 3a_ 11.png|200px]] [[File:tigre 6.17 3a_ 08.png|200px]] |
| | [[File:tigre 6.17 3a_ 20.png|200px]] [[File:tigre 6.17 3a_ 21.png|200px]] |
| | [[File:tigre 6.17 3a_ 22.png|200px]] |
| | |
| | |- |
| | | width ="30"| Gasses |
| | |C<sub>4</sub>F<sub>8</sub> 50 sccm, SF<sub>6</sub> 0 sccm |
| | |- |
| | | Pressure |
| | |10 mTorr |
| | |- |
| | | Powers |
| | |500 W Coil |
| | |- |
| | | rowspan="4"| Etch step (boost) |
| | |Duration |
| | |1.5 s |
| | |- |
| | | Gasses |
| | |C<sub>4</sub>F<sub>8</sub> 0 sccm, SF<sub>6</sub> 60 sccm |
| | |- |
| | | Pressure |
| | |5 mTorr |
| | |- |
| | | Powers |
| | |400 W Coil, 50 W Platen |
| | |- |
| | |
| | | rowspan="4"| Etch step (main) |
| | |Duration |
| | |3.5 s |
| | |- |
| | | Gasses |
| | |C<sub>4</sub>F<sub>8</sub> 40 sccm, SF<sub>6</sub> 60 sccm |
| | |- |
| | | Pressure |
| | |15 mTorr |
| | |- |
| | | Powers |
| | |400 W Coil, 20 W Platen |
| | |- |
| | |
| | |Platen temperature |
| | |colspan="2"|20 °C |
| | |- |
| | |
| | ! rowspan="1" align="center"| Conditions |
| | | Conditioning |
| | |colspan="2"| Pre-clean: 10 min oxygen clean |
| | 5 min oxygen clean between runs |
| | |- |
| | ! rowspan="2" align="center"| Etch rates |
| | | Si |
| | |colspan="2"| |
| | 200 nm lines: ~700 nm/min <br> |
| | 130 nm lines: ~580 nm/min <br> |
| | |
| | |- |
| | |CSAR |
| | |colspan="2"| ~18 nm/min |
| |- | | |- |
| |} | | |} |