| Line 1: | Line 1: | ||
= Resist coating = | = Resist coating = | ||
An appropriate EBL resist must naturally be applied to the substrate. DTU Nanolab supplies a number of standard resists, please consult the table below. The default positive EBL resist is AR-P 6200.09 (CSAR). CSAR is installed on [[Specific_Process_Knowledge/Lithography/Coaters#Spin Coater: Gamma E-beam and UV|Spin Coater: Gamma E-beam and UV]] for spin coating of 2", 4" and 6" substrates. For other substrate sizes (i.e. chips) or other resists [[Specific_Process_Knowledge/Lithography/Coaters#Manual_Spin_Coaters|Spin Coater: LabSpin 02/03]] have to be used instead. The standard resist bottles are stored in the chemical cupboard in E-4. | An appropriate EBL resist must naturally be applied to the substrate. DTU Nanolab supplies a number of standard resists, please consult the table below. The default positive EBL resist is AR-P 6200.09 (CSAR). CSAR is installed on [[Specific_Process_Knowledge/Lithography/Coaters#Spin Coater: Gamma E-beam and UV|Spin Coater: Gamma E-beam and UV]] for spin coating of 2", 4" and 6" substrates. For other substrate sizes (i.e. chips) or other resists [[Specific_Process_Knowledge/Lithography/Coaters#Manual_Spin_Coaters|Spin Coater: LabSpin 02/03]] have to be used instead. The standard resist bottles are stored in the chemical cupboard in E-4. | ||
We recommend all groups or users to have their own bottle of e-beam resist inside the cleanroom. Please follow the [[Specific Process Knowledge/Lithography/EBeamLithography/ResistBottles|user resist bottles in the cleanroom guide.]] | We recommend all groups or users to have their own bottle of e-beam resist inside the cleanroom. Please follow the [[Specific Process Knowledge/Lithography/EBeamLithography/ResistBottles|user resist bottles in the cleanroom guide.]] | ||
==DTU Nanolab supplied EBL resists== | ==DTU Nanolab supplied EBL resists== | ||
<br> | |||
{|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" width="95%" | {|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" width="95%" | ||
|- | |- | ||
| Line 63: | Line 61: | ||
|Negative | |Negative | ||
|[http://www.allresist.com AllResist] | |[http://www.allresist.com AllResist] | ||
|[[media:AR- | |[[media:AR-N-7520New.pdf|AR-N7500New]] | ||
|[[Specific_Process_Knowledge/Lithography/Coaters#Manual_Spin_Coaters|Spin Coater: LabSpin 02/03]] | |[[Specific_Process_Knowledge/Lithography/Coaters#Manual_Spin_Coaters|Spin Coater: LabSpin 02/03]] | ||
|PGMEA | |PGMEA | ||
| Line 102: | Line 100: | ||
|} | |} | ||
<br> | |||
<br> | |||
==User supplied resists== | ==User supplied resists== | ||
It is possible to obtain permission to user other resists at DTU Nanolab, users must however provide these resists and possibly developers themselves. A non-exhaustive list of user supplied EBL resist used at DTU Nanolab and some process guidelines can be found in the table below. | It is possible to obtain permission to user other resists at DTU Nanolab, users must however provide these resists and possibly developers themselves. A non-exhaustive list of user supplied EBL resist used at DTU Nanolab and some process guidelines can be found in the table below. | ||
<br> | |||
{|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" width="95%" | {|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" width="95%" | ||
|- | |- | ||
| Line 146: | Line 145: | ||
|- | |- | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
|'''[[ | |'''[[Specific Process Knowledge/Lithography/EBeamLithography/AR-P 617|Copolymer AR-P 617]]''' | ||
|Positive | |Positive | ||
|[http://www.allresist.com AllResist] | |[http://www.allresist.com AllResist] | ||
| Line 160: | Line 159: | ||
|- | |- | ||
|-style="background:LightGrey; color:black" | |-style="background:LightGrey; color:black" | ||
|''' | |'''mr EBL 6000.1''' | ||
|Negative | |Negative | ||
|[http://http://www.microresist.de/home_en.htm MicroResist] | |[http://http://www.microresist.de/home_en.htm MicroResist] | ||
| Line 185: | Line 184: | ||
| | | | ||
|[[media:Process Flow HSQ.docx|process flow HSQ]] | |[[media:Process Flow HSQ.docx|process flow HSQ]] | ||
|- | |- | ||
|-style="background:LightGrey; color:black" | |-style="background:LightGrey; color:black" | ||
|''' | |'''AR-N 7500 <br> (not "New" Series)''' | ||
|Negative | |Negative | ||
|[http://www.allresist.com AllResist] | |[http://www.allresist.com AllResist] | ||
|[https://www.allresist.com/wp-content/uploads/sites/2/2020/03/AR-N7500_english_Allresist_product-information.pdf AR-N 7500 | |[https://www.allresist.com/wp-content/uploads/sites/2/2020/03/AR-N7500_english_Allresist_product-information.pdf AR-N 7500] | ||
|[[Specific_Process_Knowledge/Lithography/Coaters#Manual_Spin_Coaters|Spin Coater: LabSpin 02/03]] | |[[Specific_Process_Knowledge/Lithography/Coaters#Manual_Spin_Coaters|Spin Coater: LabSpin 02/03]] | ||
|a = 17126, b = -0.435 | |a = 17126, b = -0.435 | ||