Jump to content

Specific Process Knowledge/Etch/DryEtchProcessing/Comparison: Difference between revisions

From LabAdviser
Jmli (talk | contribs)
No edit summary
Bghe (talk | contribs)
No edit summary
 
(53 intermediate revisions by 2 users not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Etch/DryEtchProcessing/Comparison click here]'''  
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/DryEtchProcessing/Comparison click here]'''  
<!--Checked for updates on 14/5-2018 - ok/jmli -->
<!--Checked for updates on 14/5-2018 - ok/jmli -->


== Hardware and option comparison of the dry etchers at Danchip ==
== Hardware and option comparison of the dry etchers ==
{{Template:Contentbydryetch}}
<!--Checked for updates on 3/2-2023 - ok/jmli -->


The table below compares the hardware and the options.
The table below compares the hardware and the options.


{| border="2" cellspacing="0" cellpadding="0" align="center"  
 
 
{| border="2" cellspacing="0" cellpadding="0" align="left"  
! colspan="2" style="background:silver; color:black" rowspan="2" |
! colspan="2" style="background:silver; color:black" rowspan="2" |
! style="background:silver; color:black" rowspan="2" | [[Specific Process Knowledge/Etch/ASE_(Advanced_Silicon_Etch)| ASE]]
! style="background:silver; color:black" rowspan="2" align="center" | [[Specific Process Knowledge/Etch/ASE_(Advanced_Silicon_Etch)| ASE]]
! style="background:silver; color:black" rowspan="2" | [[Specific Process Knowledge/Etch/AOE_(Advanced_Oxide_Etch)| AOE]]
! style="background:silver; color:black" rowspan="2"  align="center"| [[Specific Process Knowledge/Etch/AOE_(Advanced_Oxide_Etch)| AOE]]
! style="background:silver; color:black" colspan="2" | [[Specific Process Knowledge/Etch/DRIE-Pegasus| DRIE-Pegasus]]
! style="background:silver; color:black" colspan="4" align="center"| [[Specific Process Knowledge/Etch/DRIE-Pegasus| DRIE-Pegasi]]
! style="background:silver; color:black" rowspan="2" | [[Specific Process Knowledge/Etch/ICP_Metal_Etcher| ICP Metal etch ]]
! style="background:silver; color:black" rowspan="2"  align="center"| [[Specific Process Knowledge/Etch/ICP_Metal_Etcher| ICP Metal etch ]]
! style="background:silver; color:black" rowspan="2" | [[Specific Process Knowledge/Etch/III-V RIE |III-V RIE ]]
! style="background:silver; color:black" rowspan="2"  align="center"| [[Specific Process Knowledge/Etch/III-V ICP|III-V ICP]]
! style="background:silver; color:black" rowspan="2" | [[Specific Process Knowledge/Etch/III-V ICP|III-V ICP]]
! style="background:silver; color:black" rowspan="2"  align="center"| [[Specific Process Knowledge/Etch/IBE&frasl;IBSD Ionfab 300|IBE/IBSD Ionfab 300]]
|- valign="top"
|- valign="top"
! [[Specific_Process_Knowledge/Etch/DRIE-Pegasus/Pegasus-1|Pegasus 1]]   
! style="background:silver; color:black"  align="center"| [[Specific_Process_Knowledge/Etch/DRIE-Pegasus/Pegasus-1|Pegasus 1]]   
! [[Specific_Process_Knowledge/Etch/DRIE-Pegasus/Pegasus-2|Pegasus 2]]
! style="background:silver; color:black"  align="center"| [[Specific_Process_Knowledge/Etch/DRIE-Pegasus/Pegasus-2|Pegasus 2]]
! style="background:silver; color:black" align="center"| [[Specific_Process_Knowledge/Etch/DRIE-Pegasus/Pegasus-3|Pegasus 3]] 
! style="background:silver; color:black" align="center"| [[Specific_Process_Knowledge/Etch/DRIE-Pegasus/Pegasus-4|Pegasus 4]]
|- valign="top"
|- valign="top"
! rowspan="2" style="background:silver; color:black" width="120" |Purpose
! rowspan="2" style="background:silver; color:black" |Purpose
! style="background:WhiteSmoke; color:black" | Primary uses
! style="background:WhiteSmoke; color:black" | Primary uses
| style="background:WhiteSmoke; color:black"| Formerly the primary silicon etcher; now polymers, Silicon oxides and nitrides may also be etched. 5% metal on the surface is allowed.
| style="background:WhiteSmoke; color:black"| Formerly the primary silicon etcher; now polymers, Silicon oxides and nitrides may also be etched. 5% metal on the surface is allowed.
| style="background:WhiteSmoke; color:black"| Etching of silicon oxides or nitrides
| style="background:WhiteSmoke; color:black"| Etching of silicon oxides or nitrides on 4" wafers
| style="background:WhiteSmoke; color:black"| Silicon etching
| style="background:WhiteSmoke; color:black"| Silicon etching of 4" wafers
| style="background:WhiteSmoke; color:black"| Standard recipes for etching of Al, Cr and Ti, now also etches of W, TiW and Mo
| style="background:WhiteSmoke; color:black"| Research tool into silicon etching - only a few special recipes!
| style="background:WhiteSmoke; color:black"| Etching of silicon oxide, resist, BCB, silicon nitride, InP, InGaAs and GaAs on III-V substrates
| style="background:WhiteSmoke; color:black"| Silicon etching of 6" wafers on 6" wafers
| style="background:WhiteSmoke; color:black"| Etching of III-V materials such as GaN, InP/InGaAsP/InGaAs, AlGaAs, GaAs
| style="background:WhiteSmoke; color:black"| Etching of silicon oxides or nitrides on 6" wafers
 
| style="background:WhiteSmoke; color:black"| Standard recipes for etching of Al, Cr and Ti, now also etches of W, TiW and Mo. Please do not use this machine with F-chemistry unless the Dry Etch group has allowed it!
| style="background:WhiteSmoke; color:black"| Etching of III-V materials such as GaN, InP/InGaAsP/InGaAs, AlGaAs, GaAs.
Etching of SiO2 and SiN on III-V materials
| style="background:WhiteSmoke; color:black"| Physical Etching of all materials
|- valign="top"
|- valign="top"
! style="background:lightgrey; color:black" | Alternative/backup uses
! style="background:lightgrey; color:black" | Alternative or backup uses
| style="background:lightgrey; color:black" | Backup silicon etcher
| style="background:lightgrey; color:black" |  
| style="background:lightgrey; color:black" |  
| style="background:lightgrey; color:black" |  
| style="background:lightgrey; color:black" | Barc etch
| style="background:lightgrey; color:black" | Silicon etcher
| style="background:lightgrey; color:black" |  
| style="background:lightgrey; color:black" |  
| style="background:lightgrey; color:black" |  
| style="background:lightgrey; color:black" |  
 
| style="background:lightgrey; color:black" colspan="2"|
| style="background:lightgrey; color:black" |
| style="background:lightgrey; color:black" |
| style="background:lightgrey; color:black" |
|- valign="top"
|- valign="top"
! rowspan="7" style="background:silver; color:black" | General description
! rowspan="7" style="background:silver; color:black" | General description
Line 41: Line 51:
| style="background:WhiteSmoke; color:black" |  Inductively coupled plasma chamber with two RF generators; the coil and platen generator
| style="background:WhiteSmoke; color:black" |  Inductively coupled plasma chamber with two RF generators; the coil and platen generator
| style="background:WhiteSmoke; color:black" |  Inductively coupled plasma chamber with two RF generators; the coil and platen generator
| style="background:WhiteSmoke; color:black" |  Inductively coupled plasma chamber with two RF generators; the coil and platen generator
| style="background:WhiteSmoke; color:black" | Inductively coupled plasma chamber with two RF generators; the coil (with outer and inner coil) and platen generator
| style="background:WhiteSmoke; color:black" colspan="4" | Inductively coupled plasma chamber with two RF generators; the coil (with outer and inner coil) and platen generator
| style="background:WhiteSmoke; color:black" | Inductively coupled plasma chamber with two RF generators; the coil and platen generator
| style="background:WhiteSmoke; color:black" | Inductively coupled plasma chamber with two RF generators; the coil and platen generator
| style="background:WhiteSmoke; color:black" | Parallel plate capacitor setup with RF power between the two electrodes
| style="background:WhiteSmoke; color:black" | Inductively coupled plasma chamber with two RF generators; the coil and platen generator
| style="background:WhiteSmoke; color:black" | Inductively coupled plasma chamber with two RF generators; the coil and platen generator
 
| style="background:WhiteSmoke; color:black" | Ion beam etcher - sputter etches with argon ions


|-valign="top"
|-valign="top"
! style="background:lightgrey; color:black" | Substrate cooling/temperature
! style="background:lightgrey; color:black" | Substrate cooling and temperature
| style="background:lightgrey; color:black" | The electrode is oil cooled. Also, Helium backside cooling: -10<sup>o</sup>C to 20<sup>o</sup>C  
| style="background:lightgrey; color:black" | The electrode is oil cooled. Also, Helium backside cooling: -10<sup>o</sup>C to 20<sup>o</sup>C  
| style="background:lightgrey; color:black" | The electrode is oil cooled. Also, Helium backside cooling: -10<sup>o</sup>C to 60<sup>o</sup>C  
| style="background:lightgrey; color:black" | The electrode is oil cooled. Also, Helium backside cooling: -10<sup>o</sup>C to 60<sup>o</sup>C  
| style="background:lightgrey; color:black" | The electrode is oil cooled. Also, Helium backside cooling: -20<sup>o</sup>C to 30<sup>o</sup>C  
| style="background:lightgrey; color:black" colspan="4" | The electrode is oil cooled. Also, Helium backside cooling: -20<sup>o</sup>C to 30<sup>o</sup>C  
| style="background:lightgrey; color:black" | The electrode is oil cooled. Also, Helium backside cooling: -10<sup>o</sup>C to 50<sup>o</sup>C  
| style="background:lightgrey; color:black" | The electrode is oil cooled. Also, Helium backside cooling: -10<sup>o</sup>C to 50<sup>o</sup>C  
| style="background:lightgrey; color:black" | The electrode is oil cooled: Fixed at 20<sup>o</sup>C
| style="background:lightgrey; color:black" | The electrode is oil cooled with a special chiller. Also, Helium backside cooling: 20<sup>o</sup>C to 180<sup>o</sup>C  
| style="background:lightgrey; color:black" | The electrode is oil cooled with a special chiller. Also, Helium backside cooling: 20<sup>o</sup>C to 180<sup>o</sup>C  
| style="background:lightgrey; color:black" | The electrode is oil cooled with a special chiller. Also, Helium backside cooling: 5<sup>o</sup>C to 60?<sup>o</sup>C


|-valign="top"
|-valign="top"
! style="background:WhiteSmoke; color:black" | Clamping
! style="background:WhiteSmoke; color:black" | Clamping and wafer size
| style="background:WhiteSmoke; color:black" | Electrostatic clamping (semco electrode)
| style="background:WhiteSmoke; color:black" | Electrostatic clamping (semco electrode)<br> Wafer size 4"
| style="background:WhiteSmoke; color:black" | Electrostatic clamping (TDESC)
| style="background:WhiteSmoke; color:black" | Electrostatic clamping (TDESC)<br> Wafer size 4"
| style="background:WhiteSmoke; color:black" | Electrostatic clamping (TDESC)
| style="background:WhiteSmoke; color:black" | Electrostatic clamping (TDESC)<br> Wafer size 4"
| style="background:WhiteSmoke; color:black" | Electrostatic clamping (TDESC)
| style="background:WhiteSmoke; color:black" colspan="3" | Electrostatic clamping (TDESC)<br> Wafer size 6"
| style="background:WhiteSmoke; color:black" | No clamping
| style="background:WhiteSmoke; color:black" | Electrostatic clamping (TDESC)<br> Wafer size 6"
| style="background:WhiteSmoke; color:black" | Mechanical clamping (weighted clamp with ceramic fingers)
| style="background:WhiteSmoke; color:black" | Mechanical clamping (weighted clamp with ceramic fingers)<br> Wafer size 4"
 
| style="background:WhiteSmoke; color:black" | Mechanical clamping <br> Wafer sizes 2"/4"/6"/8"
|-valign="top"
|-valign="top"
! style="background:lightgrey; color:black" | Gasses
! style="background:lightgrey; color:black" | Gasses
Line 97: Line 106:
| Ar
| Ar
|}
|}
| style="background:lightgrey; color:black" |  
|style="background:lightgrey; color:black" |
{|
| SF<sub>6</sub>
| O<sub>2</sub>
| N<sub>2</sub>
|-
| Ar
| He
|}
|style="background:lightgrey; color:black" |
{|
| SF<sub>6</sub>
| O<sub>2</sub>
| C<sub>4</sub>F<sub>8</sub>
|-
| Ar
|}
|style="background:lightgrey; color:black" |  
{|
{|
| SF<sub>6</sub>
| SF<sub>6</sub>
Line 104: Line 130:
|-
|-
| Ar
| Ar
| He
| CF<sub>4</sub>
| CF<sub>4</sub>
| H<sub>2</sub>
|-
| BCl<sub>3</sub>
| Cl<sub>2</sub>
| HBr
|}
|}
| style="background:lightgrey; color:black" |  
| style="background:lightgrey; color:black" |  
{|
{|
| SF<sub>6</sub>
| O<sub>2</sub>
| O<sub>2</sub>
| CHF<sub>3</sub>
| C<sub>4</sub>F<sub>8</sub>
| CH<sub>4</sub>
|-
|-
| Ar
| Ar
| CF<sub>4</sub>
| H<sub>2</sub>
| H<sub>2</sub>
|-
| BCl<sub>3</sub>
| Cl<sub>2</sub>
| HBr
|}
|}
| style="background:lightgrey; color:black" |  
| style="background:lightgrey; color:black" |  
Line 133: Line 162:
| BCl<sub>3</sub>
| BCl<sub>3</sub>
| Cl<sub>2</sub>
| Cl<sub>2</sub>
|N<sub>2</sub>
|}
| style="background:lightgrey; color:black" |
{|
| Ar
| O<sub>2</sub>
| CHF<sub>3</sub>
|}
|}


Line 143: Line 179:
* Coil generator
* Coil generator
* Platen generator
* Platen generator
|  style="background:WhiteSmoke; color:black" |  
|  style="background:WhiteSmoke; color:black"|
* Coil generator
* Platen generator
* Low frequency platen generator
|  style="background:WhiteSmoke; color:black"|
* Platen generator
* Low frequency platen generator
|  style="background:WhiteSmoke; color:black" colspan="2"|  
* Coil generator
* Coil generator
* Platen generator
* Platen generator
Line 150: Line 193:
* Coil generator
* Coil generator
* Platen generator
* Platen generator
|  style="background:WhiteSmoke; color:black" |
* RF generator
|  style="background:WhiteSmoke; color:black" |  
|  style="background:WhiteSmoke; color:black" |  
* Coil generator
* Coil generator
* Platen generator
* Platen generator
|  style="background:WhiteSmoke; color:black" |
* Coil generator on plama chamber
* 3 accelerator grids between plasma chamber and process chamber


|-valign="top"
|-valign="top"
Line 162: Line 206:
| style="background:lightgrey; color:black" | Loading via dedicated two-slot carousel load lock or via atmospheric cassette loader
| style="background:lightgrey; color:black" | Loading via dedicated two-slot carousel load lock or via atmospheric cassette loader
| style="background:lightgrey; color:black" | Loading via dedicated two-slot carousel load lock
| style="background:lightgrey; color:black" | Loading via dedicated two-slot carousel load lock
| style="background:lightgrey; color:black" | Manual loading directly into process chamber
| style="background:lightgrey; color:black" colspan="2"| Loading via two cassette loading stations pumped down at vacuum
| style="background:lightgrey; color:black" | Loading via dedicated two-slot carousel load lock
| style="background:lightgrey; color:black" | Loading via dedicated two-slot carousel load lock
 
| style="background:lightgrey; color:black" | Loading via dedicated two-slot carousel load lock
| style="background:lightgrey; color:black" | Automatic loading via load lock
|-valign="top"
|-valign="top"
!  style="background:WhiteSmoke; color:black" | Options
!  style="background:WhiteSmoke; color:black" | Options
Line 172: Line 217:
|  style="background:WhiteSmoke; color:black" |  
|  style="background:WhiteSmoke; color:black" |  
|  style="background:WhiteSmoke; color:black" |  
|  style="background:WhiteSmoke; color:black" |  
* Bosch multiplexing
* Parameter ramping
* SOI option
* Claritas endpoint detection
|  style="background:WhiteSmoke; color:black"|
* Bosch multiplexing
* Bosch multiplexing
* Parameter ramping
* Parameter ramping
Line 177: Line 227:
* Optical endpoint detection
* Optical endpoint detection
|  style="background:WhiteSmoke; color:black" |  
|  style="background:WhiteSmoke; color:black" |  
* Bosch multiplexing
* Parameter ramping
* Parameter ramping
* SOI option
* Optical endpoint detection
* Optical endpoint detection
|  style="background:WhiteSmoke; color:black" |  
|  style="background:WhiteSmoke; color:black" |  
* Laser endpoint detection
* Bosch multiplexing
* Parameter ramping
* SOI option
|  style="background:WhiteSmoke; color:black" |
* Parameter ramping
* Optical endpoint detection
|  style="background:WhiteSmoke; color:black" |  
|  style="background:WhiteSmoke; color:black" |  
* Parameter ramping
* Parameter ramping
Line 186: Line 243:
* Optical endpoint detection
* Optical endpoint detection
* Laser endpoint detection
* Laser endpoint detection
|  style="background:WhiteSmoke; color:black" |
* SIMS endpoint detection
|-valign="top"
|-valign="top"
! style="background:silver; color:black"| Allowed materials
 
! style="background:silver; color:black" rowspan="2"| Allowed materials
! style="background:lightgrey; color:black" | Materials
| style="background:lightgrey; color:black" |  
| style="background:lightgrey; color:black" |  
| style="background:lightgrey; color:black" |
* Silicon, Silicon oxide, silicon nitride
* Silicon
* Fused silica
* Fused silica
* Sapphire
* Sapphire
* SiC
* SiC
* Resists
* Some polymers
* Some polymers
*<5% metal on the suface (for 4")
*<5% metal on the suface (for 4")
| style="background:lightgrey; color:black" |  
| style="background:lightgrey; color:black" |  
* Silicon
* Silicon, Silicon oxide, silicon nitride
* Fused silica
* Fused silica
* Sapphire
* Sapphire
* SiC
* SiC
| style="background:lightgrey; color:black" |
* Resists
* Silicon
* Al,(Cr) as masking materials
| style="background:lightgrey; color:black" colspan="4"|
* Silicon, Silicon oxide, silicon nitride
* Fused silica
* Fused silica
* Sapphire
* Sapphire
* SiC
* SiC
* Resists
| style="background:lightgrey; color:black" |  
| style="background:lightgrey; color:black" |  
* Silicon
* Silicon, Silicon oxide, silicon nitride
* Fused silica
* Fused silica
* Sapphire
* Sapphire
* SiC
* SiC
* Al, Cr, Ti, W, Mo, Nb
* Resists
| style="background:lightgrey; color:black" |  
| style="background:lightgrey; color:black" |  
* Silicon
* Silicon, Silicon oxide, silicon nitride
* Fused silica
* Aluminium
* Sapphire
* SiC
* GaAs, GaN, InP, with epitaxial layers
| style="background:lightgrey; color:black" |
* Silicon
* Fused silica
* Fused silica
* Sapphire
* Sapphire
* SiC
* SiC
* GaAs, GaN, InP, with epitaxial layers
* GaAs, GaN, InP, with epitaxial layers
* Resists (at low temperature processing)
|style="background:lightgrey; color:black" |
* Almost any material
|-
! style="background:WhiteSmoke; color:black" | Cross contamination sheet
| style="background:WhiteSmoke; color:black" | [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=105 Link]
| style="background:WhiteSmoke; color:black" | [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=115 Link]
| style="background:WhiteSmoke; color:black" | [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=265 Link]
| style="background:WhiteSmoke; color:black" | [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=398 Link]
| style="background:WhiteSmoke; color:black" | [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=455 Link]
| style="background:WhiteSmoke; color:black" | [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=456 Link]
| style="background:WhiteSmoke; color:black" | [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=266 Link]
| style="background:WhiteSmoke; color:black" | [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=268 Link]
| style="background:WhiteSmoke; color:black" | [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=267 Link]
|-
|-
|}
|}

Latest revision as of 11:58, 2 February 2026

Feedback to this page: click here

Hardware and option comparison of the dry etchers

Unless otherwise stated, the content of this page was created by the dry etch group at DTU Nanolab

The table below compares the hardware and the options.


ASE AOE DRIE-Pegasi ICP Metal etch III-V ICP IBE/IBSD Ionfab 300
Pegasus 1 Pegasus 2 Pegasus 3 Pegasus 4
Purpose Primary uses Formerly the primary silicon etcher; now polymers, Silicon oxides and nitrides may also be etched. 5% metal on the surface is allowed. Etching of silicon oxides or nitrides on 4" wafers Silicon etching of 4" wafers Research tool into silicon etching - only a few special recipes! Silicon etching of 6" wafers on 6" wafers Etching of silicon oxides or nitrides on 6" wafers Standard recipes for etching of Al, Cr and Ti, now also etches of W, TiW and Mo. Please do not use this machine with F-chemistry unless the Dry Etch group has allowed it! Etching of III-V materials such as GaN, InP/InGaAsP/InGaAs, AlGaAs, GaAs.

Etching of SiO2 and SiN on III-V materials

Physical Etching of all materials
Alternative or backup uses
General description Plasma source Inductively coupled plasma chamber with two RF generators; the coil and platen generator Inductively coupled plasma chamber with two RF generators; the coil and platen generator Inductively coupled plasma chamber with two RF generators; the coil (with outer and inner coil) and platen generator Inductively coupled plasma chamber with two RF generators; the coil and platen generator Inductively coupled plasma chamber with two RF generators; the coil and platen generator Ion beam etcher - sputter etches with argon ions
Substrate cooling and temperature The electrode is oil cooled. Also, Helium backside cooling: -10oC to 20oC The electrode is oil cooled. Also, Helium backside cooling: -10oC to 60oC The electrode is oil cooled. Also, Helium backside cooling: -20oC to 30oC The electrode is oil cooled. Also, Helium backside cooling: -10oC to 50oC The electrode is oil cooled with a special chiller. Also, Helium backside cooling: 20oC to 180oC The electrode is oil cooled with a special chiller. Also, Helium backside cooling: 5oC to 60?oC
Clamping and wafer size Electrostatic clamping (semco electrode)
Wafer size 4"
Electrostatic clamping (TDESC)
Wafer size 4"
Electrostatic clamping (TDESC)
Wafer size 4"
Electrostatic clamping (TDESC)
Wafer size 6"
Electrostatic clamping (TDESC)
Wafer size 6"
Mechanical clamping (weighted clamp with ceramic fingers)
Wafer size 4"
Mechanical clamping
Wafer sizes 2"/4"/6"/8"
Gasses
SF6 O2 C4F8
Ar CF4 CHF3 H2 He
SF6 O2 C4F8
H2 CF4 He
SF6 O2 C4F8
Ar
SF6 O2 N2
Ar He
SF6 O2 C4F8
Ar
SF6 O2 C4F8
Ar He CF4
SF6 O2 C4F8
Ar CF4 H2
BCl3 Cl2 HBr
SF6 O2 CF4
Ar CH4 H2
HBr BCl3 Cl2 N2
Ar O2 CHF3
RF generators
  • Coil generator
  • Platen generator
  • Coil generator
  • Platen generator
  • Coil generator
  • Platen generator
  • Low frequency platen generator
  • Platen generator
  • Low frequency platen generator
  • Coil generator
  • Platen generator
  • Low frequency platen generator
  • Coil generator
  • Platen generator
  • Coil generator
  • Platen generator
  • Coil generator on plama chamber
  • 3 accelerator grids between plasma chamber and process chamber
Substrate loading Loading via dedicated two-slot carousel load lock Loading via dedicated two-slot carousel load lock Loading via dedicated two-slot carousel load lock or via atmospheric cassette loader Loading via dedicated two-slot carousel load lock Loading via two cassette loading stations pumped down at vacuum Loading via dedicated two-slot carousel load lock Loading via dedicated two-slot carousel load lock Automatic loading via load lock
Options
  • Bosch multiplexing
  • Parameter ramping
  • Bosch multiplexing
  • Parameter ramping
  • SOI option
  • Claritas endpoint detection
  • Bosch multiplexing
  • Parameter ramping
  • SOI option
  • Optical endpoint detection
  • Bosch multiplexing
  • Parameter ramping
  • SOI option
  • Optical endpoint detection
  • Bosch multiplexing
  • Parameter ramping
  • SOI option
  • Parameter ramping
  • Optical endpoint detection
  • Parameter ramping
  • Bosch multiplexing
  • Optical endpoint detection
  • Laser endpoint detection
  • SIMS endpoint detection
Allowed materials Materials
  • Silicon, Silicon oxide, silicon nitride
  • Fused silica
  • Sapphire
  • SiC
  • Resists
  • Some polymers
  • <5% metal on the suface (for 4")
  • Silicon, Silicon oxide, silicon nitride
  • Fused silica
  • Sapphire
  • SiC
  • Resists
  • Al,(Cr) as masking materials
  • Silicon, Silicon oxide, silicon nitride
  • Fused silica
  • Sapphire
  • SiC
  • Resists
  • Silicon, Silicon oxide, silicon nitride
  • Fused silica
  • Sapphire
  • SiC
  • Al, Cr, Ti, W, Mo, Nb
  • Resists
  • Silicon, Silicon oxide, silicon nitride
  • Aluminium
  • Fused silica
  • Sapphire
  • SiC
  • GaAs, GaN, InP, with epitaxial layers
  • Resists (at low temperature processing)
  • Almost any material