[[Specific Process Knowledge/Lithography/Strip/plasmaAsher04_processDevelopment|Information about process development for plasma asher 04 and plasma asher 05 can be found here.]] | [[Specific Process Knowledge/Lithography/Strip/plasmaAsher04_processDevelopment|Information about process development for plasma asher 04 and plasma asher 05 can be found here.]] | ||
Latest revision as of 12:39, 12 January 2026
Plasma Asher 4

Product name: PVA Tepla Gigabatch 380M
Year of purchase: 2024
The Plasma Asher 4 can be used for the following processes:
- Photoresist stripping
- Descumming
- Surface cleaning
- Removal of organic passivation layers and masks
Plasma asher 4 has the following material restrictions:
- No metals allowed
- No metal oxides allowed
- No III-V materials allowed
The user manual, risk assessment, and contact information can be found in LabManager - requires login
Typical stripping parameters
Tested with 1.5 µm AZ 5214E on 100 mm silicon substrate.
- O2: 100 sccm
- N2: 100 sccm
- Pressure (DSC): 1.3 mbar
- Power: 1000 W
- Time (single wafer): 20-30 minutes
- Time (full boat): 90 minutes
Process development notes
Information about process development for plasma asher 04 and plasma asher 05 can be found here.