Jump to content

Specific Process Knowledge/Etch/Wet Chromium Etch: Difference between revisions

Hvje (talk | contribs)
No edit summary
Hvje (talk | contribs)
 
(5 intermediate revisions by 3 users not shown)
Line 7: Line 7:
'''All measurements on this page has been made by Nanolab staff.'''  
'''All measurements on this page has been made by Nanolab staff.'''  


[[Category: Equipment|Etch Wet Chromium]]
[[index.php?title=Category:Equipment|Etch Wet Chromium]]
[[Category: Etch (Wet) bath|Chromium]]
[[index.php?title=Category:Etch (Wet) bath|Chromium]]


==Wet etching of Chromium==
==Wet etching of Chromium==
Line 16: Line 16:
We use the following solution to etch chromium:
We use the following solution to etch chromium:


# Commercial chromium etch (Chrome Etch 18). You can see the KBA [https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhESk5HTklNVGQlYzIlODclN2N2JWMyJTgzJTdlJWMyJTg4diVjMiU4OSU3ZSVjMiU4NCVjMiU4MyVjMiU4OCU1ZVlSSQ==#K here]
# Commercial chromium etch (Chrome Etch 18). You can see the KBA (needs login) [https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhESk5HTklNVGQlYzIlODclN2N2JWMyJTgzJTdlJWMyJTg4diVjMiU4OSU3ZSVjMiU4NCVjMiU4MyVjMiU4OCU1ZVlSSQ==#K here]


The etch rate depends on the level of surface oxidation of the chromium metal, but the standard procedure (etch at room temperature: ~22°C) the Etch rate is around 150 nm/min.
The etch rate depends on the level of surface oxidation of the chromium metal, but the standard procedure (etch at room temperature: ~22°C) the Etch rate is around 150 nm/min.
PECVD SiO2 and LPCVD SiN coated wafers have been immersed in Cr etch 18 for 10min. Thickness wise: absolutely no changes (roughness after etch not measured)
Normally the etch is reused (if you etch Molybdenum never reuse), but if you need to dispose it, collect it in a bottle marked X waste.