Jump to content

Specific Process Knowledge/Etch/DRIE-Pegasus/processA: Difference between revisions

From LabAdviser
Jmli (talk | contribs)
Jmli (talk | contribs)
No edit summary
 
(21 intermediate revisions by 2 users not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/DRIE-Pegasus/processA click here]'''
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/DRIE-Pegasus/processA click here]'''
<!--Checked for updates on 2/10-2020 - ok/jmli -->
<!--Checked for updates on 2/10-2020 - ok/jmli -->
<!--Checked for updates on 28/6-2023 - ok/jmli -->
<!--Checked for updates on 21/10-2025 - ok/jmli -->
{{contentbydryetch}}


== Effects on Process A of showerhead change in December 2014 ==
== Effects on Process A of showerhead change in December 2014 ==
Line 104: Line 109:
|}
|}


== Process A acceptance test==
== Process A test==


Process A is labelled Large trench (80μm wide) 150μm depth. In the acceptance test the process was run on a 150 mm SPTS wafer with 12-13 % etch load.
Process A is intended as a wide trench (80μm wide) depth etched down some 150 µm. Below are the results from a run on a 150 mm wafer with 12-13 % etch load.


{| border="2" cellpadding="2" cellspacing="1" style="text-align:center;"
{| border="2" cellpadding="2" cellspacing="1" style="text-align:center;"
Line 229: Line 234:
|-
|-
|Etch rate in Si
|Etch rate in Si
|21 - 28 µm/min
|16 - 18.8 µm/min
|-
|-
|Non-uniformity
|Non-uniformity
Line 337: Line 342:
image:C01548.04-A.jpg|Wafer C01548.04: 35 % exposed area
image:C01548.04-A.jpg|Wafer C01548.04: 35 % exposed area
image:C01548.05-A.jpg|Wafer C01548.05: 50 % exposed area
image:C01548.05-A.jpg|Wafer C01548.05: 50 % exposed area
Without pre-etch measurements of the thicknesses of the photoresist it is not possible to determine the resist etch rate. However, it looks very uniform.
</gallery>
</gallery>
 
''Please note that without pre-etch measurements of the thicknesses of the photoresist it is not possible to determine the resist etch rate. However, it looks very uniform (batch C01548).''
<br><br>
<gallery caption="Optical images of the C01549 batch that is processed 20:10 mins." widths="250" heights="200" perrow="3">
<gallery caption="Optical images of the C01549 batch that is processed 20:10 mins." widths="250" heights="200" perrow="3">
image:C01549.01-A.jpg|Wafer C01549.01: 5 % exposed area. Some 190 nm of 600 nm oxide remains.
image:C01549.01-A.jpg|Wafer C01549.01: 5 % exposed area. Some 190 nm of 600 nm oxide remains.
Line 360: Line 365:


=== Results: SEM images of trench cross sections ===
=== Results: SEM images of trench cross sections ===


{| border="2" cellpadding="0" cellspacing="0" style="text-align:center;"
{| border="2" cellpadding="0" cellspacing="0" style="text-align:center;"
Line 368: Line 374:
! width="50" rowspan="2"| Process Information
! width="50" rowspan="2"| Process Information
! colspan="15"| SEM images of trenches
! colspan="15"| SEM images of trenches
! rowspan="2" | Numbers
|-
|-
! 2 µm
! 2 µm
Line 386: Line 391:
! 300 µm
! 300 µm
|-
|-
| January 2013
|rowspan="2"| January 2013
| Travka05, AZ 5214, '''5% open'''
|rowspan="2"| Travka05, AZ 5214, '''5% open'''
| Process A 55 cycles or 10:05 minutes, '''C01548.01'''  
|rowspan="2"| Process A 55 cycles or 10:05 minutes, '''C01548.01'''  
| [[file:C01548.01 002mu0025.jpg |75px|frameless ]]
| [[file:C01548.01 002mu0025.jpg |75px|frameless ]]
| [[file:C01548.01 003mu0026.jpg |75px|frameless ]]
| [[file:C01548.01 003mu0026.jpg |75px|frameless ]]
Line 404: Line 409:
| [[file:C01548.01 200mu0012.jpg |75px|frameless ]]
| [[file:C01548.01 200mu0012.jpg |75px|frameless ]]
| [[file:C01548.01 300mu0011.jpg |75px|frameless ]]
| [[file:C01548.01 300mu0011.jpg |75px|frameless ]]
|
|-
|colspan="15"|
{| {{table}}
{| {{table}}
| align="center" style="background:#f0f0f0;"|'''Trench width'''
| align="center" style="background:#f0f0f0;"|'''Trench width'''
Line 437: Line 443:
|}
|}
|-
|-
| January 2013
|rowspan="2"| January 2013
| Travka10, AZ 5214, '''10% open'''
|rowspan="2"| Travka10, AZ 5214, '''10% open'''
| Process A 55 cycles or 10:05 minutes, '''C01548.02'''
|rowspan="2"| Process A 55 cycles or 10:05 minutes, '''C01548.02'''
|[[file:C01548.02 2mu  0001.jpg |75px|frameless ]]
|[[file:C01548.02 2mu  0001.jpg |75px|frameless ]]
|[[file:C01548.02 3mu  0002.jpg |75px|frameless ]]
|[[file:C01548.02 3mu  0002.jpg |75px|frameless ]]
Line 455: Line 461:
|[[file:C01548.02 200mu 0136.jpg |75px|frameless ]]
|[[file:C01548.02 200mu 0136.jpg |75px|frameless ]]
|[[file:C01548.02 300mu 0138.jpg |75px|frameless ]]
|[[file:C01548.02 300mu 0138.jpg |75px|frameless ]]
|
|-
|colspan="15"|
{| {{table}}
{| {{table}}
| align="center" style="background:#f0f0f0;"|'''Trench width (µm)'''
| align="center" style="background:#f0f0f0;"|'''Trench width (µm)'''
Line 488: Line 495:
|}  
|}  
|-
|-
| January 2013
|rowspan="2"| January 2013
| Travka20, AZ 5214, '''20% open'''
|rowspan="2"| Travka20, AZ 5214, '''20% open'''
| Process A 55 cycles or 10:05 minutes, '''C01548.03'''
|rowspan="2"| Process A 55 cycles or 10:05 minutes, '''C01548.03'''
| [[file:C01548.03 002mu0041.jpg |75px|frameless ]]
| [[file:C01548.03 002mu0041.jpg |75px|frameless ]]
| [[file:C01548.03 003mu0040.jpg |75px|frameless ]]
| [[file:C01548.03 003mu0040.jpg |75px|frameless ]]
Line 506: Line 513:
| [[file:C01548.03 200mu0028.jpg |75px|frameless ]]
| [[file:C01548.03 200mu0028.jpg |75px|frameless ]]
| [[file:C01548.03 300mu0027.jpg |75px|frameless ]]
| [[file:C01548.03 300mu0027.jpg |75px|frameless ]]
|
|-
|colspan="15"|
{| {{table}}
{| {{table}}
| align="center" style="background:#f0f0f0;"|'''Trench width (µm)'''
| align="center" style="background:#f0f0f0;"|'''Trench width (µm)'''
Line 539: Line 547:
|}
|}
|-
|-
| January 2013
|rowspan="2"| January 2013
| Travka35, AZ 5214, '''35% open'''
|rowspan="2"| Travka35, AZ 5214, '''35% open'''
| Process A 55 cycles or 10:05 minutes, '''C01548.04'''
|rowspan="2"| Process A 55 cycles or 10:05 minutes, '''C01548.04'''
| [[file:C01548.04 002mu 0042.jpg |75px|frameless ]]
| [[file:C01548.04 002mu 0042.jpg |75px|frameless ]]
| [[file:C01548.04 003mu 0043.jpg |75px|frameless ]]
| [[file:C01548.04 003mu 0043.jpg |75px|frameless ]]
Line 557: Line 565:
| [[file:C01548.04 200mu 0056.jpg |75px|frameless ]]
| [[file:C01548.04 200mu 0056.jpg |75px|frameless ]]
| [[file:C01548.04 300mu 0057.jpg |75px|frameless ]]
| [[file:C01548.04 300mu 0057.jpg |75px|frameless ]]
|
|-
|colspan="15"|
{| {{table}}
{| {{table}}
| align="center" style="background:#f0f0f0;"|'''Trench width (µm)'''
| align="center" style="background:#f0f0f0;"|'''Trench width (µm)'''
Line 590: Line 599:
|}
|}
|-
|-
| January 2013
|rowspan="2"| January 2013
| Travka50, AZ 5214, '''50% open'''
|rowspan="2"| Travka50, AZ 5214, '''50% open'''
| Process A 55 cycles or 10:05 minutes, '''C01548.05'''
|rowspan="2"| Process A 55 cycles or 10:05 minutes, '''C01548.05'''
|
|
| [[file:C01548.05 003mu 0058.jpg |75px|frameless ]]
| [[file:C01548.05 003mu 0058.jpg |75px|frameless ]]
Line 608: Line 617:
| [[file:C01548.05 200mu 0069.jpg |75px|frameless ]]
| [[file:C01548.05 200mu 0069.jpg |75px|frameless ]]
| [[file:C01548.05 300mu 0070.jpg |75px|frameless ]]
| [[file:C01548.05 300mu 0070.jpg |75px|frameless ]]
|
|-
|colspan="15"|
{| {{table}}
{| {{table}}
| align="center" style="background:#f0f0f0;"|'''Trench width (µm)'''
| align="center" style="background:#f0f0f0;"|'''Trench width (µm)'''
Line 642: Line 652:


|}
|}




Line 657: Line 664:
! width="50" rowspan="2"| Process Information
! width="50" rowspan="2"| Process Information
! colspan="15"| SEM images of trenches
! colspan="15"| SEM images of trenches
! rowspan="2" | Numbers
|-
|-
! 2 µm
! 2 µm
Line 675: Line 681:
! 300 µm
! 300 µm
|-
|-
| January 2013
|rowspan="2"| January 2013
| Travka05, 600 nm oxide, '''5% open'''
|rowspan="2"| Travka05, 600 nm oxide, '''5% open'''
| Process A 110 cycles or 20:10 minutes, '''C01549.01'''  
|rowspan="2"| Process A 110 cycles or 20:10 minutes, '''C01549.01'''  
| [[file:C01549.01 002mu 0129.jpg |75px|frameless ]]
| [[file:C01549.01 002mu 0129.jpg |75px|frameless ]]
| [[file:C01549.01 004-3mu 0128.jpg |75px|frameless ]]
| [[file:C01549.01 004-3mu 0128.jpg |75px|frameless ]]
Line 693: Line 699:
| [[file:C01549.01 200mu 0118.jpg |75px|frameless ]]
| [[file:C01549.01 200mu 0118.jpg |75px|frameless ]]
| [[file:C01549.01 300mu 0117.jpg |75px|frameless ]]
| [[file:C01549.01 300mu 0117.jpg |75px|frameless ]]
|
|-
|colspan="15"|
{| {{table}}
{| {{table}}
| align="center" style="background:#f0f0f0;"|'''Trench width (µm)'''
| align="center" style="background:#f0f0f0;"|'''Trench width (µm)'''
Line 726: Line 733:
|}
|}
|-
|-
| January 2013
|rowspan="2"| January 2013
| Travka10, 600 nm oxide, '''10% open'''
|rowspan="2"| Travka10, 600 nm oxide, '''10% open'''
| Process A 110 cycles or 20:10 minutes, '''C01549.02'''  
|rowspan="2"| Process A 110 cycles or 20:10 minutes, '''C01549.02'''  
| [[file:C01549.02 002mu 0085.jpg |75px|frameless ]]
| [[file:C01549.02 002mu 0085.jpg |75px|frameless ]]
| [[file:C01549.02 003mu 0084.jpg |75px|frameless ]]
| [[file:C01549.02 003mu 0084.jpg |75px|frameless ]]
Line 744: Line 751:
| [[file:C01549.02 200mu 0072.jpg |75px|frameless ]]
| [[file:C01549.02 200mu 0072.jpg |75px|frameless ]]
| [[file:C01549.02 300mu 0071.jpg |75px|frameless ]]
| [[file:C01549.02 300mu 0071.jpg |75px|frameless ]]
|
|-
|colspan="15"|
{| {{table}}
{| {{table}}
| align="center" style="background:#f0f0f0;"|'''Trench width (µm)'''
| align="center" style="background:#f0f0f0;"|'''Trench width (µm)'''
Line 777: Line 785:
|}
|}
|-
|-
| January 2013
|rowspan="2"| January 2013
| Travka20, 600 nm oxide, '''20% open'''
|rowspan="2"| Travka20, 600 nm oxide, '''20% open'''
| Process A 110 cycles or 20:10 minutes, '''C01549.03'''  
|rowspan="2"| Process A 110 cycles or 20:10 minutes, '''C01549.03'''  
| [[file:C01549.03 002mu 0087.jpg |75px|frameless ]]
| [[file:C01549.03 002mu 0087.jpg |75px|frameless ]]
| [[file:C01549.03 003mu 0088.jpg |75px|frameless ]]
| [[file:C01549.03 003mu 0088.jpg |75px|frameless ]]
Line 795: Line 803:
| [[file:C01549.03 200mu 0100.jpg |75px|frameless ]]
| [[file:C01549.03 200mu 0100.jpg |75px|frameless ]]
| [[file:C01549.03 300mu 0101.jpg |75px|frameless ]]
| [[file:C01549.03 300mu 0101.jpg |75px|frameless ]]
|
|-
|colspan="15"|
{| {{table}}
{| {{table}}
| align="center" style="background:#f0f0f0;"|'''Trench width (µm)'''
| align="center" style="background:#f0f0f0;"|'''Trench width (µm)'''
Line 828: Line 837:
|}
|}
|-
|-
| January 2013
|rowspan="2"| January 2013
| Travka35, 600 nm oxide, '''35% open'''
|rowspan="2"| Travka35, 600 nm oxide, '''35% open'''
| Process A 110 cycles or 20:10 minutes, '''C01549.04'''  
|rowspan="2"| Process A 110 cycles or 20:10 minutes, '''C01549.04'''  
| [[file:C01549.04 003mu 0115.jpg |75px|frameless ]]
| [[file:C01549.04 003mu 0115.jpg |75px|frameless ]]
| [[file:C01549.04 003mu 0116.jpg |75px|frameless ]]
| [[file:C01549.04 003mu 0116.jpg |75px|frameless ]]
Line 846: Line 855:
| [[file:C01549.04 200mu 0103.jpg |75px|frameless ]]
| [[file:C01549.04 200mu 0103.jpg |75px|frameless ]]
| [[file:C01549.04 300mu 0102.jpg |75px|frameless ]]
| [[file:C01549.04 300mu 0102.jpg |75px|frameless ]]
|
{| {{table}}
| align="center" style="background:#f0f0f0;"|'''Trench width (µm)'''
| align="center" style="background:#f0f0f0;"|'''2'''
| align="center" style="background:#f0f0f0;"|'''3'''
| align="center" style="background:#f0f0f0;"|'''4'''
| align="center" style="background:#f0f0f0;"|'''6'''
| align="center" style="background:#f0f0f0;"|'''8'''
| align="center" style="background:#f0f0f0;"|'''10'''
| align="center" style="background:#f0f0f0;"|'''15'''
| align="center" style="background:#f0f0f0;"|'''25'''
| align="center" style="background:#f0f0f0;"|'''40'''
| align="center" style="background:#f0f0f0;"|'''50'''
| align="center" style="background:#f0f0f0;"|'''75'''
| align="center" style="background:#f0f0f0;"|'''100'''
| align="center" style="background:#f0f0f0;"|'''150'''
| align="center" style="background:#f0f0f0;"|'''200'''
| align="center" style="background:#f0f0f0;"|'''300'''
|-
| Etched depth (µm)||||||131||146||155||164||181||205||226||234||254||264||277||284||292
|-
| Av. ER (µm/min)||||||6,5||7,2||7,7||8,2||9,0||10,2||11,2||11,6||12,6||13,1||13,8||14,1||14,5
|-
| Av. Scllp hght (nm)||||||1189||1325||1408||1495||1642||1867||2050||2125||2312||2398||2523||2584||2653
|-
| Sdwall bowing (%)||||||1,35||1,37||1,25||1,28||1,24||1,45||1,30||1,42||1,50||1,38||1,18||0,76||0,81
|-
| Sdwall angle (degs)||||||89,4||89,6||89,9||90,0||90,3||91,0||91,7||91,9||92,3||92,4||93,0||93,0||93,5
|-
| Trench width (µm)||||||8,8||11,3||13,5||16,0||21,2||31,1||46,3||56,5||81,2||108,0||157,7||210,0||310,4
|-
|}
|}
== asdfasdf ==
{| border="2" cellpadding="0" cellspacing="0" style="text-align:center;"
|+ '''Travkatesting2: Process A run for 55 cycles on travka 5, 10, 20, 35, 50 masks'''
|-
! width="30" rowspan="2" | Date
! width="40" rowspan="2"| Substrate Information
! width="50" rowspan="2"| Process Information
! colspan="15"| SEM images of trenches
! rowspan="2" | Numbers
|-
! 2 µm
! 3 µm
! 4 µm
! 6 µm
! 8 µm
! 10 µm
! 15 µm
! 25 µm
! 40 µm
! 50 µm
! 75 µm
! 100 µm
! 150 µm
! 200 µm
! 300 µm
|-
| January 2013
| Travka05, AZ 5214, '''5% open'''
| Process A 55 cycles or 10:05 minutes, '''C01548.01'''
| [[file:C01548.01 002mu0025.jpg |75px|frameless ]]
| [[file:C01548.01 003mu0026.jpg |75px|frameless ]]
| [[file:C01548.01 004mu0024.jpg |75px|frameless ]]
| [[file:C01548.01 006mu0023.jpg |75px|frameless ]]
| [[file:C01548.01 008mu0022.jpg |75px|frameless ]]
| [[file:C01548.01 010mu0021.jpg |75px|frameless ]]
| [[file:C01548.01 015mu0020.jpg |75px|frameless ]]
| [[file:C01548.01 025mu0019.jpg |75px|frameless ]]
| [[file:C01548.01 040mu0018.jpg |75px|frameless ]]
| [[file:C01548.01 050mu0016.jpg |75px|frameless ]]
| [[file:C01548.01 075mu0015.jpg |75px|frameless ]]
| [[file:C01548.01 100mu0014.jpg |75px|frameless ]]
| [[file:C01548.01 150mu0013.jpg |75px|frameless ]]
| [[file:C01548.01 200mu0012.jpg |75px|frameless ]]
| [[file:C01548.01 300mu0011.jpg |75px|frameless ]]
|
{| {{table}}
| align="center" style="background:#f0f0f0;"|'''Trench width'''
| align="center" style="background:#f0f0f0;"|'''2'''
| align="center" style="background:#f0f0f0;"|'''3'''
| align="center" style="background:#f0f0f0;"|'''4'''
| align="center" style="background:#f0f0f0;"|'''6'''
| align="center" style="background:#f0f0f0;"|'''8'''
| align="center" style="background:#f0f0f0;"|'''10'''
| align="center" style="background:#f0f0f0;"|'''15'''
| align="center" style="background:#f0f0f0;"|'''25'''
| align="center" style="background:#f0f0f0;"|'''40'''
| align="center" style="background:#f0f0f0;"|'''50'''
| align="center" style="background:#f0f0f0;"|'''75'''
| align="center" style="background:#f0f0f0;"|'''100'''
| align="center" style="background:#f0f0f0;"|'''150'''
| align="center" style="background:#f0f0f0;"|'''200'''
| align="center" style="background:#f0f0f0;"|'''300'''
|-
| Etched depth (µm)||92||106||113||126||136||146||161||181||200||208||222||230||238||243||248
|-
| Av. ER (µm/min)||9,2||10,5||11,2||12,5||13,5||14,4||16,0||18,0||19,9||20,7||22,0||22,8||23,6||24,1||24,6
|-
| Av. ER (nm/cyc)||1679||1918||2054||2294||2473||2648||2933||3299||3641||3786||4038||4184||4324||4409||4507
|-
| Sdewll bowing (%)||0,3%||0,2%||0,2%||0,3%||0,3%||0,2%||0,0%||0,2%||0,2%||-0,3%||0,1%||0,1%||0,2%||0,2%||-0,1%
|-
| Sdewll angle(degs)||90,4||90,3||90,5||90,8||90,6||90,9||91,0||90,9||90,9||91,0||90,9||90,9||91,1||91,2||91,4
|-
| Trench width (µm)||4,8||7,1||7,7||9,7||12,6||14,1||20,0||30,3||46,3||56,4||82,5||107,3||156,9||206,7||308,6
|-
|}
|-
| January 2013
| Travka10, AZ 5214, '''10% open'''
| Process A 55 cycles or 10:05 minutes, '''C01548.02'''
|[[file:C01548.02 2mu  0001.jpg |75px|frameless ]]
|[[file:C01548.02 3mu  0002.jpg |75px|frameless ]]
|[[file:C01548.02 4mu  0003.jpg |75px|frameless ]]
|[[file:C01548.02 6mu  0004.jpg |75px|frameless ]]
|[[file:C01548.02 8mu  0005.jpg |75px|frameless ]]
|[[file:C01548.02 010mu0006.jpg |75px|frameless ]]
|[[file:C01548.02 015mu0007.jpg |75px|frameless ]]
|[[file:C01548.02 025mu0008.jpg |75px|frameless ]]
|[[file:C01548.02 040mu0009.jpg |75px|frameless ]]
|[[file:C01548.02 050mu0132.jpg |75px|frameless ]]
|[[file:C01548.02 075mu0133.jpg |75px|frameless ]]
|[[file:C01548.02 100mu 0135.jpg |75px|frameless ]]
|[[file:C01548.02 150mu 0134.jpg |75px|frameless ]]
|[[file:C01548.02 200mu 0136.jpg |75px|frameless ]]
|[[file:C01548.02 300mu 0138.jpg |75px|frameless ]]
|
{| {{table}}
| align="center" style="background:#f0f0f0;"|'''Trench width (µm)'''
| align="center" style="background:#f0f0f0;"|'''2'''
| align="center" style="background:#f0f0f0;"|'''3'''
| align="center" style="background:#f0f0f0;"|'''4'''
| align="center" style="background:#f0f0f0;"|'''6'''
| align="center" style="background:#f0f0f0;"|'''8'''
| align="center" style="background:#f0f0f0;"|'''10'''
| align="center" style="background:#f0f0f0;"|'''15'''
| align="center" style="background:#f0f0f0;"|'''25'''
| align="center" style="background:#f0f0f0;"|'''40'''
| align="center" style="background:#f0f0f0;"|'''50'''
| align="center" style="background:#f0f0f0;"|'''75'''
| align="center" style="background:#f0f0f0;"|'''100'''
| align="center" style="background:#f0f0f0;"|'''150'''
| align="center" style="background:#f0f0f0;"|'''200'''
| align="center" style="background:#f0f0f0;"|'''300'''
|-
| Etched depth (µm)||90||101||108||121||130||138||152||171||189||198||210||218||228||232||239
|-
| Av. ER (µm/min)||8,9||10,0||10,7||12,0||12,9||13,7||15,1||16,9||18,8||19,6||20,9||21,6||22,6||23,1||23,7
|-
| Av. Scllp hght (nm)||1639||1834||1964||2192||2356||2508||2772||3103||3441||3601||3825||3961||4143||4227||4346
|-
| Sdwall bowing (%)||0,40||0,19||0,25||0,16||0,04||0,12||0,16||-0,18||-0,04||0,00||0,04||-0,08||-0,20||-0,05||-0,05
|-
| Sdwall angle (degs)||90,2||90,3||90,5||90,5||90,6||90,7||90,8||91,1||91,1||91,1||91,1||91,2||91,2||91,3||91,6
|-
| Trench width (µm)||5,2||7,2||8,2||10,9||13,2||15,5||20,6||31,3||46,5||56,1||81,2||107,2||158,9||211,1||306,2
|-
|}
|-
| January 2013
| Travka20, AZ 5214, '''20% open'''
| Process A 55 cycles or 10:05 minutes, '''C01548.03'''
| [[file:C01548.03 002mu0041.jpg |75px|frameless ]]
| [[file:C01548.03 003mu0040.jpg |75px|frameless ]]
| [[file:C01548.03 004mu0039.jpg |75px|frameless ]]
| [[file:C01548.03 006mu0038.jpg |75px|frameless ]]
| [[file:C01548.03 008mu0037.jpg |75px|frameless ]]
| [[file:C01548.03 010mu0036.jpg |75px|frameless ]]
| [[file:C01548.03 015mu0035.jpg |75px|frameless ]]
| [[file:C01548.03 025mu0034.jpg |75px|frameless ]]
| [[file:C01548.03 040mu0033.jpg |75px|frameless ]]
| [[file:C01548.03 050mu0032.jpg |75px|frameless ]]
| [[file:C01548.03 075mu0031.jpg |75px|frameless ]]
| [[file:C01548.03 100mu0030.jpg |75px|frameless ]]
| [[file:C01548.03 150mu0029.jpg |75px|frameless ]]
| [[file:C01548.03 200mu0028.jpg |75px|frameless ]]
| [[file:C01548.03 300mu0027.jpg |75px|frameless ]]
|
{| {{table}}
| align="center" style="background:#f0f0f0;"|'''Trench width (µm)'''
| align="center" style="background:#f0f0f0;"|'''2'''
| align="center" style="background:#f0f0f0;"|'''3'''
| align="center" style="background:#f0f0f0;"|'''4'''
| align="center" style="background:#f0f0f0;"|'''6'''
| align="center" style="background:#f0f0f0;"|'''8'''
| align="center" style="background:#f0f0f0;"|'''10'''
| align="center" style="background:#f0f0f0;"|'''15'''
| align="center" style="background:#f0f0f0;"|'''25'''
| align="center" style="background:#f0f0f0;"|'''40'''
| align="center" style="background:#f0f0f0;"|'''50'''
| align="center" style="background:#f0f0f0;"|'''75'''
| align="center" style="background:#f0f0f0;"|'''100'''
| align="center" style="background:#f0f0f0;"|'''150'''
| align="center" style="background:#f0f0f0;"|'''200'''
| align="center" style="background:#f0f0f0;"|'''300'''
|-
| Etched depth (µm)||75||85||92||103||111||117||130||148||164||170||181||188||194||199||203
|-
| Av. ER (µm/min)||7,5||8,4||9,1||10,2||11,0||11,6||12,9||14,7||16,2||16,8||17,9||18,6||19,3||19,7||20,1
|-
| Av. Scllp hght (nm)||1371||1543||1676||1874||2019||2133||2368||2692||2978||3086||3286||3412||3533||3619||3686
|-
| Sdwall bowing (%)||0,46||0,59||0,40||0,42||0,40||0,28||0,35||0,18||0,36||0,36||0,26||0,58||0,40||0,31||0,05
|-
| Sdwall angle (degs)||90,1||90,4||90,4||90,5||90,8||90,6||91,1||91,3||91,4||91,5||91,5||91,7||91,8||91,8||92,2
|-
| Trench width (µm)||4,9||6,1||7,8||10,4||12,2||14,9||19,9||30,5||46,3||57,4||82,3||106,6||158,1||209,0||309,7
|-
|}
|-
| January 2013
| Travka35, AZ 5214, '''35% open'''
| Process A 55 cycles or 10:05 minutes, '''C01548.04'''
| [[file:C01548.04 002mu 0042.jpg |75px|frameless ]]
| [[file:C01548.04 003mu 0043.jpg |75px|frameless ]]
| [[file:C01548.04 004mu 0044.jpg |75px|frameless ]]
| [[file:C01548.04 006mu 0046.jpg |75px|frameless ]]
| [[file:C01548.04 008mu 0047.jpg |75px|frameless ]]
| [[file:C01548.04 010mu 0048.jpg |75px|frameless ]]
| [[file:C01548.04 015mu 0049.jpg |75px|frameless ]]
| [[file:C01548.04 025mu 0050.jpg |75px|frameless ]]
| [[file:C01548.04 040mu 0051.jpg |75px|frameless ]]
| [[file:C01548.04 050mu 0052.jpg |75px|frameless ]]
| [[file:C01548.04 075mu 0053.jpg |75px|frameless ]]
| [[file:C01548.04 100mu 0054.jpg |75px|frameless ]]
| [[file:C01548.04 150mu 0055.jpg |75px|frameless ]]
| [[file:C01548.04 200mu 0056.jpg |75px|frameless ]]
| [[file:C01548.04 300mu 0057.jpg |75px|frameless ]]
|
{| {{table}}
| align="center" style="background:#f0f0f0;"|'''Trench width (µm)'''
| align="center" style="background:#f0f0f0;"|'''2'''
| align="center" style="background:#f0f0f0;"|'''3'''
| align="center" style="background:#f0f0f0;"|'''4'''
| align="center" style="background:#f0f0f0;"|'''6'''
| align="center" style="background:#f0f0f0;"|'''8'''
| align="center" style="background:#f0f0f0;"|'''10'''
| align="center" style="background:#f0f0f0;"|'''15'''
| align="center" style="background:#f0f0f0;"|'''25'''
| align="center" style="background:#f0f0f0;"|'''40'''
| align="center" style="background:#f0f0f0;"|'''50'''
| align="center" style="background:#f0f0f0;"|'''75'''
| align="center" style="background:#f0f0f0;"|'''100'''
| align="center" style="background:#f0f0f0;"|'''150'''
| align="center" style="background:#f0f0f0;"|'''200'''
| align="center" style="background:#f0f0f0;"|'''300'''
|-
| Etched depth (µm)||61||70||76||86||94||100||111||126||139||143||153||158||163||165||168
|-
| Av. ER (µm/min)||6,1||6,9||7,6||8,6||9,3||9,9||11,0||12,5||13,8||14,2||15,2||15,6||16,2||16,4||16,7
|-
| Av. Scllp hght (nm)||1117||1267||1390||1568||1704||1810||2014||2287||2526||2602||2786||2868||2967||3007||3054
|-
| Sdwall bowing (%)||0,22||0,31||0,30||0,46||0,39||0,55||0,41||0,20||-0,04||-0,33||-0,25||-0,19||-0,13||-0,13||-0,21
|-
| Sdwall angle (degs)||89,7||90,1||90,2||90,4||90,5||90,4||90,2||89,9||90,0||89,9||90,2||90,4||90,8||90,9||91,3
|-
| Trench width (µm)||4,5||5,4||6,7||9,0||11,4||13,4||19,1||30,0||45,0||56,2||82,3||108,4||156,3||207,5||308,3
|-
|}
|-
| January 2013
| Travka50, AZ 5214, '''50% open'''
| Process A 55 cycles or 10:05 minutes, '''C01548.05'''
|
| [[file:C01548.05 003mu 0058.jpg |75px|frameless ]]
| [[file:C01548.05 004mu 0059.jpg |75px|frameless ]]
| [[file:C01548.05 006mu 0060.jpg |75px|frameless ]]
| [[file:C01548.05 008mu 0061.jpg |75px|frameless ]]
| [[file:C01548.05 010mu 0062.jpg |75px|frameless ]]
| [[file:C01548.05 015mu 0063.jpg |75px|frameless ]]
| [[file:C01548.05 025mu 0064.jpg |75px|frameless ]]
| [[file:C01548.05 040mu 0065.jpg |75px|frameless ]]
| [[file:C01548.05 050mu 0066.jpg |75px|frameless ]]
| [[file:C01548.05 050mu 0131.jpg |75px|frameless ]]
| [[file:C01548.05 075mu 0067.jpg |75px|frameless ]]
| [[file:C01548.05 100mu 0068.jpg |75px|frameless ]]
| [[file:C01548.05 200mu 0069.jpg |75px|frameless ]]
| [[file:C01548.05 300mu 0070.jpg |75px|frameless ]]
|
{| {{table}}
| align="center" style="background:#f0f0f0;"|'''Trench width (µm)'''
| align="center" style="background:#f0f0f0;"|'''2'''
| align="center" style="background:#f0f0f0;"|'''3'''
| align="center" style="background:#f0f0f0;"|'''4'''
| align="center" style="background:#f0f0f0;"|'''6'''
| align="center" style="background:#f0f0f0;"|'''8'''
| align="center" style="background:#f0f0f0;"|'''10'''
| align="center" style="background:#f0f0f0;"|'''15'''
| align="center" style="background:#f0f0f0;"|'''25'''
| align="center" style="background:#f0f0f0;"|'''40'''
| align="center" style="background:#f0f0f0;"|'''50'''
| align="center" style="background:#f0f0f0;"|'''75'''
| align="center" style="background:#f0f0f0;"|'''100'''
| align="center" style="background:#f0f0f0;"|'''150'''
| align="center" style="background:#f0f0f0;"|'''200'''
| align="center" style="background:#f0f0f0;"|'''300'''
|-
| Etched depth (µm)||||62||67||75||81||86||94||105||113||118||123||125||129||131||133
|-
| Av. ER (µm/min)||||6,2||6,7||7,5||8,0||8,5||9,3||10,4||11,2||11,7||12,2||12,4||12,8||13,0||13,2
|-
| Av. Scllp hght (nm)||||1132||1223||1370||1472||1565||1706||1906||2061||2142||2234||2277||2355||2379||2412
|-
| Sdwall bowing (%)||||0,42||0,61||0,39||0,36||0,41||0,38||0,39||0,52||0,24||0,36||0,47||0,63||0,59||0,32
|-
| Sdwall angle (degs)||||89,9||89,8||90,0||90,1||90,5||90,7||91,1||91,3||91,6||91,8||92,1||92,3||92,4||92,6
|-
| Trench width (µm)||||5,1||6,7||9,3||11,4||13,7||18,6||29,0||44,5||54,4||80,5||106,7||156,9||207,4||310,1
|-
|}
|}
{| border="2" cellpadding="0" cellspacing="0" style="text-align:center;"
|+ '''Travkatesting2: Process A run for 110 cycles on travka 5, 10, 20, 35 masks'''
|-
! width="30" rowspan="2" | Date
! width="40" rowspan="2"| Substrate Information
! width="50" rowspan="2"| Process Information
! colspan="15"| SEM images of trenches
! rowspan="2" | Numbers
|-
! 2 µm
! 3 µm
! 4 µm
! 6 µm
! 8 µm
! 10 µm
! 15 µm
! 25 µm
! 40 µm
! 50 µm
! 75 µm
! 100 µm
! 150 µm
! 200 µm
! 300 µm
|-
| January 2013
| Travka05, 600 nm oxide, '''5% open'''
| Process A 110 cycles or 20:10 minutes, '''C01549.01'''
| [[file:C01549.01 002mu 0129.jpg |75px|frameless ]]
| [[file:C01549.01 004-3mu 0128.jpg |75px|frameless ]]
| [[file:C01549.01 004-3mu 0128.jpg |75px|frameless ]]
| [[file:C01549.01 008-6mu 0127.jpg |75px|frameless ]]
| [[file:C01549.01 008-6mu 0127.jpg |75px|frameless ]]
| [[file:C01549.01 010mu 0126.jpg |75px|frameless ]]
| [[file:C01549.01 015mu 0125.jpg |75px|frameless ]]
| [[file:C01549.01 025mu 0124.jpg |75px|frameless ]]
| [[file:C01549.01 040mu 0123.jpg |75px|frameless ]]
| [[file:C01549.01 050mu 0122.jpg |75px|frameless ]]
| [[file:C01549.01 075mu 0121.jpg |75px|frameless ]]
| [[file:C01549.01 100mu 0120.jpg |75px|frameless ]]
| [[file:C01549.01 150mu 0119.jpg |75px|frameless ]]
| [[file:C01549.01 200mu 0118.jpg |75px|frameless ]]
| [[file:C01549.01 300mu 0117.jpg |75px|frameless ]]
|
{| {{table}}
| align="center" style="background:#f0f0f0;"|'''Trench width (µm)'''
| align="center" style="background:#f0f0f0;"|'''2'''
| align="center" style="background:#f0f0f0;"|'''3'''
| align="center" style="background:#f0f0f0;"|'''4'''
| align="center" style="background:#f0f0f0;"|'''6'''
| align="center" style="background:#f0f0f0;"|'''8'''
| align="center" style="background:#f0f0f0;"|'''10'''
| align="center" style="background:#f0f0f0;"|'''15'''
| align="center" style="background:#f0f0f0;"|'''25'''
| align="center" style="background:#f0f0f0;"|'''40'''
| align="center" style="background:#f0f0f0;"|'''50'''
| align="center" style="background:#f0f0f0;"|'''75'''
| align="center" style="background:#f0f0f0;"|'''100'''
| align="center" style="background:#f0f0f0;"|'''150'''
| align="center" style="background:#f0f0f0;"|'''200'''
| align="center" style="background:#f0f0f0;"|'''300'''
|-
| Etched depth (µm)||175||195||209||229||247||260||289||330||370||393||428||454||488||507||523
|-
| Av. ER (µm/min)||8,7||9,7||10,4||11,3||12,3||12,9||14,4||16,3||18,3||19,5||21,2||22,5||24,2||25,2||25,9
|-
| Av. Scllp hght (nm)||1591||1772||1902||2079||2247||2359||2631||2997||3364||3569||3888||4124||4434||4614||4751
|-
| Sdwall bowing (%)||0,12||0,20||0,30||0,35||0,32||0,35||0,40||0,30||0,41||0,24||0,33||0,32||0,47||0,71||0,00
|-
| Sdwall angle (degs)||89,6||89,9||89,9||90,1||90,2||90,3||90,7||90,9||91,1||91,4||91,5||91,5||91,2||91,6||91,7
|-
| Trench width (µm)||8,5||9,5||10,8||13,2||16,0||18,4||22,6||33,0||48,0||57,5||82,7||106,8||159,0||207,0||306,8
|-
|}
|-
| January 2013
| Travka10, 600 nm oxide, '''10% open'''
| Process A 110 cycles or 20:10 minutes, '''C01549.02'''
| [[file:C01549.02 002mu 0085.jpg |75px|frameless ]]
| [[file:C01549.02 003mu 0084.jpg |75px|frameless ]]
| [[file:C01549.02 004mu 0083.jpg |75px|frameless ]]
| [[file:C01549.02 006mu 0082.jpg |75px|frameless ]]
| [[file:C01549.02 008mu 0081.jpg |75px|frameless ]]
| [[file:C01549.02 010mu 0080.jpg |75px|frameless ]]
| [[file:C01549.02 015mu 0079.jpg |75px|frameless ]]
| [[file:C01549.02 025mu 0078.jpg |75px|frameless ]]
| [[file:C01549.02 040mu 0077.jpg |75px|frameless ]]
| [[file:C01549.02 050mu 0076.jpg |75px|frameless ]]
| [[file:C01549.02 075mu 0075.jpg |75px|frameless ]]
| [[file:C01549.02 100mu 0074.jpg |75px|frameless ]]
| [[file:C01549.02 150mu 0073.jpg |75px|frameless ]]
| [[file:C01549.02 200mu 0072.jpg |75px|frameless ]]
| [[file:C01549.02 300mu 0071.jpg |75px|frameless ]]
|
{| {{table}}
| align="center" style="background:#f0f0f0;"|'''Trench width (µm)'''
| align="center" style="background:#f0f0f0;"|'''2'''
| align="center" style="background:#f0f0f0;"|'''3'''
| align="center" style="background:#f0f0f0;"|'''4'''
| align="center" style="background:#f0f0f0;"|'''6'''
| align="center" style="background:#f0f0f0;"|'''8'''
| align="center" style="background:#f0f0f0;"|'''10'''
| align="center" style="background:#f0f0f0;"|'''15'''
| align="center" style="background:#f0f0f0;"|'''25'''
| align="center" style="background:#f0f0f0;"|'''40'''
| align="center" style="background:#f0f0f0;"|'''50'''
| align="center" style="background:#f0f0f0;"|'''75'''
| align="center" style="background:#f0f0f0;"|'''100'''
| align="center" style="background:#f0f0f0;"|'''150'''
| align="center" style="background:#f0f0f0;"|'''200'''
| align="center" style="background:#f0f0f0;"|'''300'''
|-
| Etched depth (µm)||164||179||190||209||224||238||263||300||337||358||388||404||438||452||469
|-
| Av. ER (µm/min)||8,1||8,9||9,4||10,4||11,1||11,8||13,1||14,9||16,7||17,7||19,2||20,0||21,7||22,4||23,2
|-
| Av. Scllp hght (nm)||1489||1626||1730||1899||2034||2163||2395||2724||3063||3251||3526||3671||3978||4110||4262
|-
| Sdwall bowing (%)||0,20||0,41||0,46||0,57||0,74||0,62||0,68||0,75||0,58||0,99||0,54||0,49||0,72||0,51||0,77
|-
| Sdwall angle (degs)||89,7||90,0||89,9||90,1||90,2||90,3||90,8||91,2||91,5||91,3||92,0||92,2||92,6||92,8||93,6
|-
| Trench width (µm)||7,9||8,7||10,4||12,6||16,1||18,1||22,8||33,5||49,3||58,1||83,1||108,6||157,0||207,1||301,3
|-
|}
|-
| January 2013
| Travka20, 600 nm oxide, '''20% open'''
| Process A 110 cycles or 20:10 minutes, '''C01549.03'''
| [[file:C01549.03 002mu 0087.jpg |75px|frameless ]]
| [[file:C01549.03 003mu 0088.jpg |75px|frameless ]]
| [[file:C01549.03 004mu 0089.jpg |75px|frameless ]]
| [[file:C01549.03 006mu 0090.jpg |75px|frameless ]]
| [[file:C01549.03 008mu 0091.jpg |75px|frameless ]]
| [[file:C01549.03 010mu 0092.jpg |75px|frameless ]]
| [[file:C01549.03 015mu 0093.jpg |75px|frameless ]]
| [[file:C01549.03 025mu 0094.jpg |75px|frameless ]]
| [[file:C01549.03 040mu 0095.jpg |75px|frameless ]]
| [[file:C01549.03 050mu 0096.jpg |75px|frameless ]]
| [[file:C01549.03 075mu 0097.jpg |75px|frameless ]]
| [[file:C01549.03 100mu 0098.jpg |75px|frameless ]]
| [[file:C01549.03 150mu 0099.jpg |75px|frameless ]]
| [[file:C01549.03 200mu 0100.jpg |75px|frameless ]]
| [[file:C01549.03 300mu 0101.jpg |75px|frameless ]]
|
{| {{table}}
| align="center" style="background:#f0f0f0;"|'''Trench width (µm)'''
| align="center" style="background:#f0f0f0;"|'''2'''
| align="center" style="background:#f0f0f0;"|'''3'''
| align="center" style="background:#f0f0f0;"|'''4'''
| align="center" style="background:#f0f0f0;"|'''6'''
| align="center" style="background:#f0f0f0;"|'''8'''
| align="center" style="background:#f0f0f0;"|'''10'''
| align="center" style="background:#f0f0f0;"|'''15'''
| align="center" style="background:#f0f0f0;"|'''25'''
| align="center" style="background:#f0f0f0;"|'''40'''
| align="center" style="background:#f0f0f0;"|'''50'''
| align="center" style="background:#f0f0f0;"|'''75'''
| align="center" style="background:#f0f0f0;"|'''100'''
| align="center" style="background:#f0f0f0;"|'''150'''
| align="center" style="background:#f0f0f0;"|'''200'''
| align="center" style="background:#f0f0f0;"|'''300'''
|-
| Etched depth (µm)||142||153||164||181||195||206||228||258||287||303||326||342||366||380||392
|-
| Av. ER (µm/min)||7,0||7,6||8,1||9,0||9,7||10,2||11,3||12,8||14,2||15,0||16,2||17,0||18,2||18,8||19,4
|-
| Av. Scllp hght (nm)||1288||1390||1493||1647||1775||1877||2073||2342||2612||2754||2967||3108||3331||3451||3561
|-
| Sdwall bowing (%)||0,54||0,77||1,08||0,83||1,06||0,91||0,95||1,07||0,88||0,75||0,95||0,05||0,83||0,73||0,46
|-
| Sdwall angle (degs)||89,6||89,6||89,8||90,2||90,3||90,6||90,9||91,5||91,6||91,8||92,3||93,3||92,5||92,9||93,0
|-
| Trench width (µm)||7,2||8,7||9,9||12,4||14,7||16,9||22,8||31,1||48,4||58,0||81,9||108,6||160,4||209,9||311,1
|-
|}
|-
|-
| January 2013
|colspan="15"|
| Travka35, 600 nm oxide, '''35% open'''
| Process A 110 cycles or 20:10 minutes, '''C01549.04'''
| [[file:C01549.04 003mu 0115.jpg |75px|frameless ]]
| [[file:C01549.04 003mu 0116.jpg |75px|frameless ]]
| [[file:C01549.04 004mu 0114.jpg |75px|frameless ]]
| [[file:C01549.04 006mu 0113.jpg |75px|frameless ]]
| [[file:C01549.04 008mu 0112.jpg |75px|frameless ]]
| [[file:C01549.04 010mu 0111.jpg |75px|frameless ]]
| [[file:C01549.04 015mu 0110.jpg |75px|frameless ]]
| [[file:C01549.04 025mu 0109.jpg |75px|frameless ]]
| [[file:C01549.04 040mu 0108.jpg |75px|frameless ]]
| [[file:C01549.04 050mu 0107.jpg |75px|frameless ]]
| [[file:C01549.04 075mu 0106.jpg |75px|frameless ]]
| [[file:C01549.04 100mu 0105.jpg |75px|frameless ]]
| [[file:C01549.04 150mu 0104.jpg |75px|frameless ]]
| [[file:C01549.04 200mu 0103.jpg |75px|frameless ]]
| [[file:C01549.04 300mu 0102.jpg |75px|frameless ]]
|
{| {{table}}
{| {{table}}
| align="center" style="background:#f0f0f0;"|'''Trench width (µm)'''
| align="center" style="background:#f0f0f0;"|'''Trench width (µm)'''

Latest revision as of 11:41, 21 October 2025

Feedback to this page: click here


Unless otherwise stated, the content of this page was created by the dry etch group at DTU Nanolab

Effects on Process A of showerhead change in December 2014

The effects of changing of the showerhead in December 2014 was investigated. Patterned wafers were processed before and after and the profile of the etched features were inspected in SEM. Click on the numbers in the 'Runs' column below to see the profiles.


Recipe Name Temp. Deposition step Etch step Comments
Time Pres. C4F8 SF6 O2 Coil Time Pres. C4F8 SF6 O2 Coil Platen Showerhead Runs Key words
Process A Step1 11 cyc 20 4 25 200 0 0 2000 7.0 25(1.5s) 90>>150 0 350(1.5s) 550 5 2800 120>>140(1.5s) 45 Old 1
Step2 44 cyc 4 25 200 0 0 2000 7.0 25(1.5s) 150 0 350(1.5s) 550 5 2800 140(1.5s) 45
Step1 11 cyc 20 4 25 200 0 0 2000 7.0 25(1.5s) 90>>150 0 350(1.5s) 550 5 2800 120>>140(1.5s) 45 New 1 Profile improved
Step2 44 cyc 4 25 200 0 0 2000 7.0 25(1.5s) 150 0 350(1.5s) 550 5 2800 140(1.5s) 45

Process A test

Process A is intended as a wide trench (80μm wide) depth etched down some 150 µm. Below are the results from a run on a 150 mm wafer with 12-13 % etch load.

Process A specifications
Parameter Specification Average result
Etch rate (µm/min) > 15 18.9
Etched depth (µm) 150 189.1
Scallop size (nm) < 800 718
Profile (degs) 91 +/- 1 91.1
Selectivity to AZ photoresist > 150 310
Undercut (µm) <1.5 0.84
Uniformity (%) < 3.5 3.0
Repeatability (%) <4 0.43


Process A parameters
Step 1 Step 2
Parameter Etch Dep Etch Dep
Gas flow (sccm) SF6 350 (1.5 s) 550 C4F8 200 SF6 350 (1.5 s) 550 C4F8 200
Cycle time (secs) 7.0 4.0 7.0 4.0
Pressure (mtorr) 25 (1.5 s) 90 >> 150 25 25 (1.5 s) 150 25
Coil power (W) 2800 2000 2800 2000
Platen power (W) 120 >> 140 (1.5) 45 0 140 (1.5) 45 0
Cycles 11 (keep fixed) 44 (vary this)
Common Temperature 20 degs, HBC 10 torr, Short funnel, with baffle & 5mm spacers

Quality control procedure

Quality Control (QC) for DRIE-Pegasus
QC Recipe: Process A
Step 1: 11 cycles Step 2: 44 cycles
QC limits DRIE-Pegasus
Etch rate in Si 16 - 18.8 µm/min
Non-uniformity 2  %

Process A guidelines

Process A is optimized for speed and depending on feature size and etch load it will achieve etch rates up to 25-30 µm/min.

This aggressive etch has a few drawbacks - one of which is the release of energy in the etch process. In general, it is clear that

  1. The higher the etch rate, the higher rate of released energy.
  2. The larger an area of silicon is exposed to plasma and hence etched, the higher rate of released energy.

Given its high etch rate, Process A is very sensible to high etch load processes and substrates with reduced cooling efficiency. Therefore, users are generally advised to

  1. Use Process A with precaution at high etch loads - above some 50%.
  2. Avoid using Process A on bonded wafers, in particular if the etch load is more than 5-10%. The bonding reduces the heat conduction across the wafer interface so the top wafer will immediately heat up and cause the mask to erode and the bonding polymer to melt.

If you have a bonded sandwich of wafers with very poor heat conduction (typically caused by intermediate polymer layers thicker than a few microns) you are advised to use other etch processes, maybe the deepetch on the ASE.

Process A performance

The perfomance of Process A has been investigated as a function of feature size and etch load.

Experiment

A number of wafers are patterned with the Travka mask set in AZ photoresist or 600 nm oxide. The wafers are then etched (batch recipe with 5 minute TDESC interstep cleans) using two different durations of process A in the DRIE-Pegasus.

Wafers
Wafer number Mask Mask material Process A duration
C01548.01 Travka 05 AZ photoresist 55 cycles, 10:05 mins
C01548.02 Travka 10 AZ photoresist 55 cycles, 10:05 mins
C01548.03 Travka 20 AZ photoresist 55 cycles, 10:05 mins
C01548.04 Travka 35 AZ photoresist 55 cycles, 10:05 mins
C01548.05 Travka 50 AZ photoresist 55 cycles, 10:05 mins
Wafers
Wafer number Mask Mask material Process A duration
C01549.01 Travka 05 600 nm oxide 110 cycles, 20:10 mins
C01549.02 Travka 10 600 nm oxide 110 cycles, 20:10 mins
C01549.03 Travka 20 600 nm oxide 110 cycles, 20:10 mins
C01549.04 Travka 35 600 nm oxide 110 cycles, 20:10 mins

Results: Optical images

Please note that without pre-etch measurements of the thicknesses of the photoresist it is not possible to determine the resist etch rate. However, it looks very uniform (batch C01548).

The etching of silicon releases energy. This means that the faster the etch is, the more heat needs to be dissipated. The consequence is the same if a larger percentage of the wafer is etched. Process A is the fastest etch and as seen above, the exposed area plays an important role. As the exposed area increases the oxide mask erosion is more and more pronounced.

If a larger area is to be etched, the cooling must be made more efficient, either by lowering the platen temperature or with increasing the pressure of He on the backside of the wafer. This will be investigated soon.

Results: Etched depths in trenches of different widths

Results: SEM images of trench cross sections

Travkatesting2: Process A run for 55 cycles on travka 5, 10, 20, 35, 50 masks
Date Substrate Information Process Information SEM images of trenches
2 µm 3 µm 4 µm 6 µm 8 µm 10 µm 15 µm 25 µm 40 µm 50 µm 75 µm 100 µm 150 µm 200 µm 300 µm
January 2013 Travka05, AZ 5214, 5% open Process A 55 cycles or 10:05 minutes, C01548.01
Trench width 2 3 4 6 8 10 15 25 40 50 75 100 150 200 300
Etched depth (µm) 92 106 113 126 136 146 161 181 200 208 222 230 238 243 248
Av. ER (µm/min) 9,2 10,5 11,2 12,5 13,5 14,4 16,0 18,0 19,9 20,7 22,0 22,8 23,6 24,1 24,6
Av. ER (nm/cyc) 1679 1918 2054 2294 2473 2648 2933 3299 3641 3786 4038 4184 4324 4409 4507
Sdewll bowing (%) 0,3% 0,2% 0,2% 0,3% 0,3% 0,2% 0,0% 0,2% 0,2% -0,3% 0,1% 0,1% 0,2% 0,2% -0,1%
Sdewll angle(degs) 90,4 90,3 90,5 90,8 90,6 90,9 91,0 90,9 90,9 91,0 90,9 90,9 91,1 91,2 91,4
Trench width (µm) 4,8 7,1 7,7 9,7 12,6 14,1 20,0 30,3 46,3 56,4 82,5 107,3 156,9 206,7 308,6
January 2013 Travka10, AZ 5214, 10% open Process A 55 cycles or 10:05 minutes, C01548.02
Trench width (µm) 2 3 4 6 8 10 15 25 40 50 75 100 150 200 300
Etched depth (µm) 90 101 108 121 130 138 152 171 189 198 210 218 228 232 239
Av. ER (µm/min) 8,9 10,0 10,7 12,0 12,9 13,7 15,1 16,9 18,8 19,6 20,9 21,6 22,6 23,1 23,7
Av. Scllp hght (nm) 1639 1834 1964 2192 2356 2508 2772 3103 3441 3601 3825 3961 4143 4227 4346
Sdwall bowing (%) 0,40 0,19 0,25 0,16 0,04 0,12 0,16 -0,18 -0,04 0,00 0,04 -0,08 -0,20 -0,05 -0,05
Sdwall angle (degs) 90,2 90,3 90,5 90,5 90,6 90,7 90,8 91,1 91,1 91,1 91,1 91,2 91,2 91,3 91,6
Trench width (µm) 5,2 7,2 8,2 10,9 13,2 15,5 20,6 31,3 46,5 56,1 81,2 107,2 158,9 211,1 306,2
January 2013 Travka20, AZ 5214, 20% open Process A 55 cycles or 10:05 minutes, C01548.03
Trench width (µm) 2 3 4 6 8 10 15 25 40 50 75 100 150 200 300
Etched depth (µm) 75 85 92 103 111 117 130 148 164 170 181 188 194 199 203
Av. ER (µm/min) 7,5 8,4 9,1 10,2 11,0 11,6 12,9 14,7 16,2 16,8 17,9 18,6 19,3 19,7 20,1
Av. Scllp hght (nm) 1371 1543 1676 1874 2019 2133 2368 2692 2978 3086 3286 3412 3533 3619 3686
Sdwall bowing (%) 0,46 0,59 0,40 0,42 0,40 0,28 0,35 0,18 0,36 0,36 0,26 0,58 0,40 0,31 0,05
Sdwall angle (degs) 90,1 90,4 90,4 90,5 90,8 90,6 91,1 91,3 91,4 91,5 91,5 91,7 91,8 91,8 92,2
Trench width (µm) 4,9 6,1 7,8 10,4 12,2 14,9 19,9 30,5 46,3 57,4 82,3 106,6 158,1 209,0 309,7
January 2013 Travka35, AZ 5214, 35% open Process A 55 cycles or 10:05 minutes, C01548.04
Trench width (µm) 2 3 4 6 8 10 15 25 40 50 75 100 150 200 300
Etched depth (µm) 61 70 76 86 94 100 111 126 139 143 153 158 163 165 168
Av. ER (µm/min) 6,1 6,9 7,6 8,6 9,3 9,9 11,0 12,5 13,8 14,2 15,2 15,6 16,2 16,4 16,7
Av. Scllp hght (nm) 1117 1267 1390 1568 1704 1810 2014 2287 2526 2602 2786 2868 2967 3007 3054
Sdwall bowing (%) 0,22 0,31 0,30 0,46 0,39 0,55 0,41 0,20 -0,04 -0,33 -0,25 -0,19 -0,13 -0,13 -0,21
Sdwall angle (degs) 89,7 90,1 90,2 90,4 90,5 90,4 90,2 89,9 90,0 89,9 90,2 90,4 90,8 90,9 91,3
Trench width (µm) 4,5 5,4 6,7 9,0 11,4 13,4 19,1 30,0 45,0 56,2 82,3 108,4 156,3 207,5 308,3
January 2013 Travka50, AZ 5214, 50% open Process A 55 cycles or 10:05 minutes, C01548.05
Trench width (µm) 2 3 4 6 8 10 15 25 40 50 75 100 150 200 300
Etched depth (µm) 62 67 75 81 86 94 105 113 118 123 125 129 131 133
Av. ER (µm/min) 6,2 6,7 7,5 8,0 8,5 9,3 10,4 11,2 11,7 12,2 12,4 12,8 13,0 13,2
Av. Scllp hght (nm) 1132 1223 1370 1472 1565 1706 1906 2061 2142 2234 2277 2355 2379 2412
Sdwall bowing (%) 0,42 0,61 0,39 0,36 0,41 0,38 0,39 0,52 0,24 0,36 0,47 0,63 0,59 0,32
Sdwall angle (degs) 89,9 89,8 90,0 90,1 90,5 90,7 91,1 91,3 91,6 91,8 92,1 92,3 92,4 92,6
Trench width (µm) 5,1 6,7 9,3 11,4 13,7 18,6 29,0 44,5 54,4 80,5 106,7 156,9 207,4 310,1



Travkatesting2: Process A run for 110 cycles on travka 5, 10, 20, 35 masks
Date Substrate Information Process Information SEM images of trenches
2 µm 3 µm 4 µm 6 µm 8 µm 10 µm 15 µm 25 µm 40 µm 50 µm 75 µm 100 µm 150 µm 200 µm 300 µm
January 2013 Travka05, 600 nm oxide, 5% open Process A 110 cycles or 20:10 minutes, C01549.01
Trench width (µm) 2 3 4 6 8 10 15 25 40 50 75 100 150 200 300
Etched depth (µm) 175 195 209 229 247 260 289 330 370 393 428 454 488 507 523
Av. ER (µm/min) 8,7 9,7 10,4 11,3 12,3 12,9 14,4 16,3 18,3 19,5 21,2 22,5 24,2 25,2 25,9
Av. Scllp hght (nm) 1591 1772 1902 2079 2247 2359 2631 2997 3364 3569 3888 4124 4434 4614 4751
Sdwall bowing (%) 0,12 0,20 0,30 0,35 0,32 0,35 0,40 0,30 0,41 0,24 0,33 0,32 0,47 0,71 0,00
Sdwall angle (degs) 89,6 89,9 89,9 90,1 90,2 90,3 90,7 90,9 91,1 91,4 91,5 91,5 91,2 91,6 91,7
Trench width (µm) 8,5 9,5 10,8 13,2 16,0 18,4 22,6 33,0 48,0 57,5 82,7 106,8 159,0 207,0 306,8
January 2013 Travka10, 600 nm oxide, 10% open Process A 110 cycles or 20:10 minutes, C01549.02
Trench width (µm) 2 3 4 6 8 10 15 25 40 50 75 100 150 200 300
Etched depth (µm) 164 179 190 209 224 238 263 300 337 358 388 404 438 452 469
Av. ER (µm/min) 8,1 8,9 9,4 10,4 11,1 11,8 13,1 14,9 16,7 17,7 19,2 20,0 21,7 22,4 23,2
Av. Scllp hght (nm) 1489 1626 1730 1899 2034 2163 2395 2724 3063 3251 3526 3671 3978 4110 4262
Sdwall bowing (%) 0,20 0,41 0,46 0,57 0,74 0,62 0,68 0,75 0,58 0,99 0,54 0,49 0,72 0,51 0,77
Sdwall angle (degs) 89,7 90,0 89,9 90,1 90,2 90,3 90,8 91,2 91,5 91,3 92,0 92,2 92,6 92,8 93,6
Trench width (µm) 7,9 8,7 10,4 12,6 16,1 18,1 22,8 33,5 49,3 58,1 83,1 108,6 157,0 207,1 301,3
January 2013 Travka20, 600 nm oxide, 20% open Process A 110 cycles or 20:10 minutes, C01549.03
Trench width (µm) 2 3 4 6 8 10 15 25 40 50 75 100 150 200 300
Etched depth (µm) 142 153 164 181 195 206 228 258 287 303 326 342 366 380 392
Av. ER (µm/min) 7,0 7,6 8,1 9,0 9,7 10,2 11,3 12,8 14,2 15,0 16,2 17,0 18,2 18,8 19,4
Av. Scllp hght (nm) 1288 1390 1493 1647 1775 1877 2073 2342 2612 2754 2967 3108 3331 3451 3561
Sdwall bowing (%) 0,54 0,77 1,08 0,83 1,06 0,91 0,95 1,07 0,88 0,75 0,95 0,05 0,83 0,73 0,46
Sdwall angle (degs) 89,6 89,6 89,8 90,2 90,3 90,6 90,9 91,5 91,6 91,8 92,3 93,3 92,5 92,9 93,0
Trench width (µm) 7,2 8,7 9,9 12,4 14,7 16,9 22,8 31,1 48,4 58,0 81,9 108,6 160,4 209,9 311,1
January 2013 Travka35, 600 nm oxide, 35% open Process A 110 cycles or 20:10 minutes, C01549.04
Trench width (µm) 2 3 4 6 8 10 15 25 40 50 75 100 150 200 300
Etched depth (µm) 131 146 155 164 181 205 226 234 254 264 277 284 292
Av. ER (µm/min) 6,5 7,2 7,7 8,2 9,0 10,2 11,2 11,6 12,6 13,1 13,8 14,1 14,5
Av. Scllp hght (nm) 1189 1325 1408 1495 1642 1867 2050 2125 2312 2398 2523 2584 2653
Sdwall bowing (%) 1,35 1,37 1,25 1,28 1,24 1,45 1,30 1,42 1,50 1,38 1,18 0,76 0,81
Sdwall angle (degs) 89,4 89,6 89,9 90,0 90,3 91,0 91,7 91,9 92,3 92,4 93,0 93,0 93,5
Trench width (µm) 8,8 11,3 13,5 16,0 21,2 31,1 46,3 56,5 81,2 108,0 157,7 210,0 310,4