Jump to content

Specific Process Knowledge/Etch/Etching of Bulk Glass: Difference between revisions

Jmli (talk | contribs)
Bghe (talk | contribs)
 
(3 intermediate revisions by 2 users not shown)
Line 1: Line 1:
'''Unless anything else is stated, everything on this page, text and pictures are made by DTU Nanolab.'''
'''All links to Kemibrug (SDS) and Labmanager Including APV and QC requires login.'''
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/Etching_of_Bulk_Glass click here]'''
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/Etching_of_Bulk_Glass click here]'''
<!-- Replace "http://labadviser.nanolab.dtu.dk/..." with the link to the Labadviser page-->
<!-- Replace "http://labadviser.nanolab.dtu.dk/..." with the link to the Labadviser page-->
Line 4: Line 8:
== Comparing methods for etching bulk glass at DTU Nanolab ==
== Comparing methods for etching bulk glass at DTU Nanolab ==


Etching of glass can be done either wet or dry. Wet etching is done with HF. Dry etching can be done either with [[Specific Process Knowledge/Etch/AOE (Advanced Oxide Etch)|AOE]] using fluorine chemistry (only fused silica) or with [[Specific Process Knowledge/Etch/IBE⁄IBSD Ionfab 300|IBE]] by sputtering with Ar ions and/or using fluorine chemistry.  
Etching of glass can be done either wet or dry. Wet etching is done with HF. Dry etching can be done either with [[Specific Process Knowledge/Etch/AOE (Advanced Oxide Etch)|AOE]], ASE or Pegasus 4 using fluorine chemistry (only fused silica) or with [[Specific Process Knowledge/Etch/IBE⁄IBSD Ionfab 300|IBE]] by sputtering with Ar ions and/or using fluorine chemistry.  


At DTU Nanolab, we have two types of bulk glass substrates: Borosilicate glass (Borofloat 33 (like pyrex)) and fused silica glass which in cleanliness is similar to quartz. Both types are etched wet in a special set-up placed in a fumehood using a concentrated HF-solution (isotropic etch).
At DTU Nanolab, we have two types of bulk glass substrates: Borosilicate glass (Borofloat 33 (like pyrex)) and fused silica glass which in cleanliness is similar to quartz. Both types are etched wet in a special set-up placed in a fumehood using a concentrated HF-solution (isotropic etch).
Line 80: Line 84:
|
|
*~75 nm/min (Thermal oxide) in BHF
*~75 nm/min (Thermal oxide) in BHF
*~90 nm/min (Thermal oxide) in SIO Etch
*~80 nm/min (Thermal oxide) in BOE 7:1 Etchant VLSI with Surfactant
*~25 nm/min (Thermal oxide) in 5%HF
*~25 nm/min (Thermal oxide) in 5%HF
*~3-4µm/min in 40%HF