'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/IBE⁄IBSD_Ionfab_300/IBE_blazed_gratings click here]''' | '''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/IBE⁄IBSD_Ionfab_300/IBE_blazed_gratings click here]''' | ||
<br> {{CC-bghe1}} | |||
*60 nm Barc | |||
*360 nm KRF resist | |||
''by bghe@nanolab'' experiments made in June/July 2012 | |||
<gallery widths="300px" heights="250px" caption="Some examples of blazed gratings in fused silica etched with Cr and DUV resist as masking layer"> | |||
Image:IBE 30min -Cr1.jpg |'''30 min etch with 100 nm Cr mask, used recipe BGHE blazed gratings with CHF3''' <br>*Rotation speed 0 rpm<br>*Angle: -35<br>*I(N) = 400 mA<br>*RF power = 1300 W<br>*I(B) = 300 mA<br>*V(B) = 300 V<br>*V(AC,B)=500 V<br>*Ar(N) flow = 5 sccm<br>*Ar(B) flow = 5 sccm<br>*CHF3 flow = 15 sccm | |||
Image:after IBE 45min_A_34.jpg |'''45min etch with 100nm Cr mask, used recipe BGHE blazed gratings with CHF3''' <br>*Rotation speed 0 rpm<br>*Angle: -35<br>*I(N) = 400 mA<br>*RF power = 1300 W<br>*I(B) = 300 mA<br>*V(B) = 300 V<br>*V(AC,B) = 500 V<br>*Ar(N) flow = 5 sccm<br>*Ar(B) flow = 5 sccm<br>*CHF3 flow = 15 sccm | |||
Image:Edge_1.jpg|'''20min etch with Krf resist, all resist is gone, used recipe BGHE blazed gratings''' <br>*Rotation speed 0 rpm<br>*Angle: -35<br>*I(N) = 550 mA<br>*RF power = 1300 W<br>*I(B) = 500 mA<br>*V(B) = 600 V<br>*V(AC,B) = 400 V<br>*Ar(N) flow = 5 sccm<br>*Ar(B) flow = 10 sccm<br>*CHF3 flow = 0 sccm | |||
Image:15min+30min5.jpg|'''15+30min etch with 50nm Cr mask, used recipe BGHE blazed gratings with CHF3''' <br>*Rotation speed 0 rpm<br>*Angle: -35<br>*I(N) = 400 mA<br>*RF power = 1300 W<br>*I(B) = 300 mA<br>*V(B) = 300 V<br>*V(AC,B) = 500 V<br>*Ar(N) flow = 5 sccm<br>*Ar(B) flow = 5 sccm<br>*CHF3 flow = 15 sccm | |||
</gallery> | </gallery> | ||
Latest revision as of 10:25, 4 September 2025
Feedback to this page: click here
The content on this page, including all images and pictures, was created by Berit Herstrøm @ DTU Nanolab (BGHE), unless otherwise stated.
- 60 nm Barc
- 360 nm KRF resist
by bghe@nanolab experiments made in June/July 2012
- Some examples of blazed gratings in fused silica etched with Cr and DUV resist as masking layer
-
30 min etch with 100 nm Cr mask, used recipe BGHE blazed gratings with CHF3
*Rotation speed 0 rpm
*Angle: -35
*I(N) = 400 mA
*RF power = 1300 W
*I(B) = 300 mA
*V(B) = 300 V
*V(AC,B)=500 V
*Ar(N) flow = 5 sccm
*Ar(B) flow = 5 sccm
*CHF3 flow = 15 sccm -
45min etch with 100nm Cr mask, used recipe BGHE blazed gratings with CHF3
*Rotation speed 0 rpm
*Angle: -35
*I(N) = 400 mA
*RF power = 1300 W
*I(B) = 300 mA
*V(B) = 300 V
*V(AC,B) = 500 V
*Ar(N) flow = 5 sccm
*Ar(B) flow = 5 sccm
*CHF3 flow = 15 sccm -
20min etch with Krf resist, all resist is gone, used recipe BGHE blazed gratings
*Rotation speed 0 rpm
*Angle: -35
*I(N) = 550 mA
*RF power = 1300 W
*I(B) = 500 mA
*V(B) = 600 V
*V(AC,B) = 400 V
*Ar(N) flow = 5 sccm
*Ar(B) flow = 10 sccm
*CHF3 flow = 0 sccm -
15+30min etch with 50nm Cr mask, used recipe BGHE blazed gratings with CHF3
*Rotation speed 0 rpm
*Angle: -35
*I(N) = 400 mA
*RF power = 1300 W
*I(B) = 300 mA
*V(B) = 300 V
*V(AC,B) = 500 V
*Ar(N) flow = 5 sccm
*Ar(B) flow = 5 sccm
*CHF3 flow = 15 sccm