=Etch slow (this was tested in 2012 by ''bghe@nanolab'')= | |||
This process development | This process development was done to find an etch recipe that is so gentle that the resist masking material can be removed with acetone + ultrasound within hopefully 10 min. This is important when a Cr is to be etched as this cannot withstand plasma ashing (to remove the resist mask) after the etch. All though it is tested on silicon the recipe can be used ofr other material giving slightly different etch rates. | ||
{| border="2" cellspacing="2" cellpadding="3" | {| border="2" cellspacing="2" cellpadding="3" | ||
!Parameter | !Parameter | ||
!Si etch | !Si etch test1 | ||
!Si etch test2 | |||
!Si etch test3 | |||
|- | |||
!Important note | |||
| | |||
|This recipe must only be run for 5 min, otherwise the beam acc. current will incrase above 20 | |||
| | |||
|- | |- | ||
|Neutalizer current [mA] | |Neutalizer current [mA] | ||
|450 | |||
|250 | |||
|450 | |450 | ||
|- | |- | ||
|RF Power [W] | |RF Power [W] | ||
|1200 | |||
|1000 | |||
|1200 | |1200 | ||
|- | |- | ||
|Beam current [mA] | |Beam current [mA] | ||
|400 | |||
|200 | |||
|400 | |400 | ||
|- | |- | ||
|Beam voltage [V] | |Beam voltage [V] | ||
|400 | |||
|200 | |||
|400 | |400 | ||
|- | |- | ||
|Beam accelerator voltage | |Beam accelerator voltage | ||
|400 | |||
|200 | |||
|400 | |400 | ||
|- | |- | ||
|Ar flow to neutralizer [sccm] | |Ar flow to neutralizer [sccm] | ||
|6.0 | |||
|6.0 | |||
|6.0 | |6.0 | ||
|- | |- | ||
|Ar flow to beam [sccm] | |Ar flow to beam [sccm] | ||
|6.0 | |||
|6.0 | |||
|6.0 | |6.0 | ||
|- | |- | ||
|Rotation speed [rpm] | |Rotation speed [rpm] | ||
|20 | |||
|20 | |||
|20 | |20 | ||
|- | |- | ||
|Stage angle [degrees] | |Stage angle [degrees] | ||
|10 | |||
|10 | |||
|10 | |10 | ||
|- | |- | ||
|Platen temp. [dg. Celcius] | |Platen temp. [dg. Celcius] | ||
|15 | |||
|15 | |||
|15 | |15 | ||
|- | |- | ||
|He cooling pressure [mTorr] | |He cooling pressure [mTorr] | ||
|37.5 | |37.5 | ||
|37.5 | |||
|37.5 | |||
|- | |||
|Etch material | |||
|Si | |||
|Si | |||
|Si | |||
|- | |- | ||
|'''Results''' | |'''Results''' | ||
|'''vvv''' | |||
|'''vvv''' | |||
|'''vvv''' | |'''vvv''' | ||
|- | |- | ||
| | |Etch time [min] | ||
|40 | |||
|40 | |40 | ||
|7:15 | |||
|- | |- | ||
|Etch rate in Si [nm/min] | |Etch rate in Si [nm/min] | ||
|19.7 | |19.7 | ||
|3.58 | |||
|19.3 | |||
|- | |- | ||
|Total time in Acetone + ultrasound [min] | |Total time in Acetone + ultrasound [min] | ||
|17 | |17 | ||
|10 | |||
|20 | |||
|- | |- | ||
|Was the resist completely removed after acetone + ultrasound? | |Was the resist completely removed after acetone + ultrasound? | ||
|no | |no | ||
|yes | |||
|yes (almost) | |||
|- | |- | ||
|} | |} | ||
Latest revision as of 11:15, 4 September 2025
Feedback to this page: click here
The content on this page, including all images and pictures, was created by Berit Herstrøm @ DTU Nanolab (BGHE), unless otherwise stated.
Etch slow (this was tested in 2012 by bghe@nanolab)
This process development was done to find an etch recipe that is so gentle that the resist masking material can be removed with acetone + ultrasound within hopefully 10 min. This is important when a Cr is to be etched as this cannot withstand plasma ashing (to remove the resist mask) after the etch. All though it is tested on silicon the recipe can be used ofr other material giving slightly different etch rates.
| Parameter | Si etch test1 | Si etch test2 | Si etch test3 |
|---|---|---|---|
| Important note | This recipe must only be run for 5 min, otherwise the beam acc. current will incrase above 20 | ||
| Neutalizer current [mA] | 450 | 250 | 450 |
| RF Power [W] | 1200 | 1000 | 1200 |
| Beam current [mA] | 400 | 200 | 400 |
| Beam voltage [V] | 400 | 200 | 400 |
| Beam accelerator voltage | 400 | 200 | 400 |
| Ar flow to neutralizer [sccm] | 6.0 | 6.0 | 6.0 |
| Ar flow to beam [sccm] | 6.0 | 6.0 | 6.0 |
| Rotation speed [rpm] | 20 | 20 | 20 |
| Stage angle [degrees] | 10 | 10 | 10 |
| Platen temp. [dg. Celcius] | 15 | 15 | 15 |
| He cooling pressure [mTorr] | 37.5 | 37.5 | 37.5 |
| Etch material | Si | Si | Si |
| Results | vvv | vvv | vvv |
| Etch time [min] | 40 | 40 | 7:15 |
| Etch rate in Si [nm/min] | 19.7 | 3.58 | 19.3 |
| Total time in Acetone + ultrasound [min] | 17 | 10 | 20 |
| Was the resist completely removed after acetone + ultrasound? | no | yes | yes (almost) |