Jump to content

Specific Process Knowledge/Characterization/XPS/XPS technique: Difference between revisions

From LabAdviser
Jmli (talk | contribs)
Jmli (talk | contribs)
No edit summary
 
(49 intermediate revisions by the same user not shown)
Line 1: Line 1:
 
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Characterization/XPS/XPS_technique click here]'''
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php?title=Specific_Process_Knowledge/Characterization/XPS/XPS_technique click here]'''
<!-- Page reviewed 9/8-2022 jmli -->
 
<!-- Page reviewed 8/5-2023 jmli -->
{{Author-jmli1}}
<!--Checked for updates on 4/9-2025 - ok/jmli -->


=XPS technique=
=XPS technique=


XPS is a surface sensitive and non destructive technique used for analysis of the elemental composition of a sample. It relies on the photoelectric effect; X-ray photons irradiated onto a sample will cause electrons bound in the sample atoms to become free electrons inside the the sample. The kinetic energy of these photoelectrons depend on the energy of the X-ray photon and their original binding energy. Escaping into the vacuum and counted in the electron spectrometer as function of their kinetic energy, the photoelectrons make a spectrum if represented in terms of numbers as function of their binding energy.


XPS is a surface sensitive and non destructive technique used for analysis of the elemental composition. The basic principle is shown below.
There are two reasons why the technique is extremely useful:
 
* '''Chemical sensitivity:''' The kinetic energy of the photoelectrons may be determined with such high accuracy (for instance, the resolution of the spectrometer is roughly 1 eV compared to the ~130 eV resolution of the spectrometer in an EDX X-ray detector ) that the small changes in binding energy of the sample electrons caused by the binding to other atoms may be detected. It is therefore possible to obtain information about the chemical environment of the elements - for instance in terms of:
[[File:800px-XPS_PHYSICS.jpg|600px| XPS principle (Image taken from Wikipedia)]]
** Oxidation state
 
** Double or triple bonds
In the XPS spectrometer system the probed samples are irradiated by photons with a specific energy, and the photoelectrons that leaves the sample are detected. The energy levels of the electrons are elemental specific, and by measuring the energy of the outgoing electrons, it is possible to detect which elements that are present in a sample.
** Surface states
 
* '''Surface sensitivity:''' The inelastic mean free path of the photoelectrons is very short - as a result, photoelectrons from depths larger than some 10 monolayers will not contribute to the peaks as they have lost part of their kinetic energy. This makes XPS extremely surface sensitive.
You can read further about the technique here: [http://en.wikipedia.org/wiki/X-ray_photoelectron_spectroscopy]


The basic principle is shown below. The image is taken from Wikipedia - click on it to go to the wikipedia page on X-ray photoelectron spectroscopy.


== X-ray Photoelectron Spectroscopy analysis (XPS) ==
[[File:800px-XPS_PHYSICS.jpg|700px| frameless|link=https://en.wikipedia.org/wiki/X-ray_photoelectron_spectroscopy|XPS principle. The image is taken from wikipedia - click on image to access wikipedia directly.]]


During a XPS (X-ray Photoelectron Spectroscopy) analysis, the sample is irradiated with photons of a specific energy (in the Danchip system 1486 eV). When energy of the irradiating X-rays is adsorbed by the atoms in the sample, photoelectrons are ejected [[http://en.wikipedia.org/wiki/Photoelectric_effect]].
The analysis relies on the sequence:


Since the energy of the incoming photons is known, and the energy of the ejected electrons is measured, the binding energy of the electrons in the probed atoms can be determined. The binding energy of the electrons are element specific, and is therefore a "finger-print" of the atom. Hence, a measurement of the XPS spectrum gives information of which materials are present in the sample, and at which concentrations.  
; The X-ray source
: In the X-ray gun, electrons are extracted from a filament and accelerated by a high voltage onto an aluminium anode. Here, much like the primary beam in an SEM, X-rays with the characteristic energy of aluminium (1486.7 eV) are generated. Emitted isotropically, some X-rays hit a quartz crystal that act as monochromator as the X-rays diffract on the crystal planes according to the Bragg equation. If curved, the crystal will also focus the beam of X-rays and in this way enable us to use X-ray spots (in the shape of ellipses) of different sizes - ranging from 400 µm to 40 µm. The smaller spots, however, only come at the price of a drastically lowered intensity - therefore it is generally advised only to use the default value of 400 µm unless strictly necessary for some reason.


XPS is an excellent technique to probe the chemical state of atoms on a surface. The binding energy of lower lying atomic levels (for example 1s, 2s and 2p) are at a specific energy, but is slightly affected by the chemical environment of the probed atom. This is known as the '''chemical shift'''. By measuring the shift of the electron binding energies one can determined the chemical state of atoms. See an example on the page [[Specific Process Knowledge/Characterization/XPS|XPS-ThermoScientific]].
; Generation of photoelectrons
: As the incoming and monochromatic X-rays (with energy E<sub>phot</sub>) impinge on and travel through the sample, they react with electrons bound to atoms in the sample with a certain binding energy (E<sub>bind</sub>). The result is free electron inside sample with a kinetic energy (E<sub>kin</sub>=E<sub>phot</sub>-E<sub>bind</sub>) that is characteristic of the atomic level it originated from. As the binding energy depends on the small energy changes in the electronic states induced by the formation of chemical bonds, the electron also carries information about the chemical state.


; Transport towards the vacuum
: The inelastic mean free path of the photoelectrons travelling inside a solid is very short in this energy range. The information carried by the photoelectrons will therefore quickly degrade as they collide inelastically and loose part of their energy. This means that only photoelectrons originating from the ~10 topmost atomic layers of the sample contribute to the signal - in this way making XPS extremely surface sensitive. The tail of former photoelectrons with non-specific energy is called the background. From inside the sample the electrons must pass the socalled work function in order to escape into the vacuum.


; Detection in the analyzer
: In the analyzer the electrons are separated according to the kinetic energy by two concentric spheres held at some potential. By playing on the acceptance angle of the entrance/exit slits of the analyzer one can tune the energy resolution with the parameter called the pass energy. Subsequently detected by the spectrometer, the number of electrons may be plotted as a function of energy thus making up an XPS spectrum.


=== Typical applications of XPS ===
= More information on XPS =


The XPS can be used for different applications, for example:
There is a vast number of textbooks on XPS and the internet/Youtube has plenty information as well. For the training sessions we have chosen a document entitled 'Electron Spectroscopy of surfaces' by Peter S. Deimel and Francesco Allegretti from the Technical University of Munich. It relatively short, yet thorough and takes you through theory and hardware. Skip sections 6-8. Click [[Specific_Process_Knowledge/Characterization/XPS/ExtDocs|here]] to go the page with external material.


* Do an elemental analysis of the outermost layer of your surface.
For the practical part of the training, some videos have been made. They can only be accessed using this link:
* Check the composition of a film at different depths.
*[https://www.youtube.com/playlist?list=PLjWVU97LayHBtOkPCSv8QA-sD4Dbz1jrb Youtube playlist]
* Check for a contaminations.  
** It not as sensitive as the SIMS, but faster, so it can be an alternative if you are checking for a bit higher contamination levels (like 1 %)
* Do a analysis of the chemical state of atoms present on the surface.
** See what effect a surface treatment of your sample has on the surface chemistry.
** Check a polymer covered surface. Are for example (C=O), (C-OH) (C-C) groups present in the polymer after it been deposited on a surface.

Latest revision as of 10:35, 4 September 2025

Feedback to this page: click here Unless otherwise stated, all content on this page was created by Jonas Michael-Lindhard, DTU Nanolab

XPS technique

XPS is a surface sensitive and non destructive technique used for analysis of the elemental composition of a sample. It relies on the photoelectric effect; X-ray photons irradiated onto a sample will cause electrons bound in the sample atoms to become free electrons inside the the sample. The kinetic energy of these photoelectrons depend on the energy of the X-ray photon and their original binding energy. Escaping into the vacuum and counted in the electron spectrometer as function of their kinetic energy, the photoelectrons make a spectrum if represented in terms of numbers as function of their binding energy.

There are two reasons why the technique is extremely useful:

  • Chemical sensitivity: The kinetic energy of the photoelectrons may be determined with such high accuracy (for instance, the resolution of the spectrometer is roughly 1 eV compared to the ~130 eV resolution of the spectrometer in an EDX X-ray detector ) that the small changes in binding energy of the sample electrons caused by the binding to other atoms may be detected. It is therefore possible to obtain information about the chemical environment of the elements - for instance in terms of:
    • Oxidation state
    • Double or triple bonds
    • Surface states
  • Surface sensitivity: The inelastic mean free path of the photoelectrons is very short - as a result, photoelectrons from depths larger than some 10 monolayers will not contribute to the peaks as they have lost part of their kinetic energy. This makes XPS extremely surface sensitive.

The basic principle is shown below. The image is taken from Wikipedia - click on it to go to the wikipedia page on X-ray photoelectron spectroscopy.

XPS principle. The image is taken from wikipedia - click on image to access wikipedia directly.

The analysis relies on the sequence:

The X-ray source
In the X-ray gun, electrons are extracted from a filament and accelerated by a high voltage onto an aluminium anode. Here, much like the primary beam in an SEM, X-rays with the characteristic energy of aluminium (1486.7 eV) are generated. Emitted isotropically, some X-rays hit a quartz crystal that act as monochromator as the X-rays diffract on the crystal planes according to the Bragg equation. If curved, the crystal will also focus the beam of X-rays and in this way enable us to use X-ray spots (in the shape of ellipses) of different sizes - ranging from 400 µm to 40 µm. The smaller spots, however, only come at the price of a drastically lowered intensity - therefore it is generally advised only to use the default value of 400 µm unless strictly necessary for some reason.
Generation of photoelectrons
As the incoming and monochromatic X-rays (with energy Ephot) impinge on and travel through the sample, they react with electrons bound to atoms in the sample with a certain binding energy (Ebind). The result is free electron inside sample with a kinetic energy (Ekin=Ephot-Ebind) that is characteristic of the atomic level it originated from. As the binding energy depends on the small energy changes in the electronic states induced by the formation of chemical bonds, the electron also carries information about the chemical state.
Transport towards the vacuum
The inelastic mean free path of the photoelectrons travelling inside a solid is very short in this energy range. The information carried by the photoelectrons will therefore quickly degrade as they collide inelastically and loose part of their energy. This means that only photoelectrons originating from the ~10 topmost atomic layers of the sample contribute to the signal - in this way making XPS extremely surface sensitive. The tail of former photoelectrons with non-specific energy is called the background. From inside the sample the electrons must pass the socalled work function in order to escape into the vacuum.
Detection in the analyzer
In the analyzer the electrons are separated according to the kinetic energy by two concentric spheres held at some potential. By playing on the acceptance angle of the entrance/exit slits of the analyzer one can tune the energy resolution with the parameter called the pass energy. Subsequently detected by the spectrometer, the number of electrons may be plotted as a function of energy thus making up an XPS spectrum.

More information on XPS

There is a vast number of textbooks on XPS and the internet/Youtube has plenty information as well. For the training sessions we have chosen a document entitled 'Electron Spectroscopy of surfaces' by Peter S. Deimel and Francesco Allegretti from the Technical University of Munich. It relatively short, yet thorough and takes you through theory and hardware. Skip sections 6-8. Click here to go the page with external material.

For the practical part of the training, some videos have been made. They can only be accessed using this link: