==The Bosch process: Etching of silicon== | ==The Bosch process: Etching of silicon== | ||
| Line 19: | Line 19: | ||
|- | |- | ||
| | | | ||
*[http://labmanager | *[http://labmanager.dtu.dk/d4Show.php?id=1607&mach=105 The QC procedure for ASE] | ||
*[http://labmanager | *[http://labmanager.dtu.dk/view_binary.php?fileId=1751 The newest QC data for ASE] | ||
{| {{table}} | {| {{table}} | ||
| Line 192: | Line 192: | ||
The recipe Iso is the same recipe as Deepetch but without the passivation steps. <br> | The recipe Iso is the same recipe as Deepetch but without the passivation steps. <br> | ||
It has been tested once by Filip Sandborg-Olsen @nanotech. <br> | It has been tested once by Filip Sandborg-Olsen @nanotech. <br> | ||
He etched with 100% load for | He etched with 100% load for 10 min. He got an etch rate of 5.51µm/min | ||
== Process development == | == Process development == | ||
===Etch of nano sized structures=== | ===Etch of nano sized structures=== | ||
{{Template:Author-bghe-thissection}} | |||
*See pxnano2 and comparison with nanotech on the Pegasus: [[Specific Process Knowledge/Etch/DRIE-Pegasus/nanoetch/nano142-pxnano2]] | *See pxnano2 and comparison with nanotech on the Pegasus: [[Specific Process Knowledge/Etch/DRIE-Pegasus/nanoetch/nano142-pxnano2]] | ||
Older work: | Older work: | ||
Three different examples of etch are shown here. The masking material was zep520A (80 nm). | Three different examples of etch are shown here. The masking material was zep520A (80 nm). | ||
{| border="1" cellspacing="1" cellpadding="2" align="left" | {| border="1" cellspacing="1" cellpadding="2" align="left" | ||
| Line 273: | Line 274: | ||
|} | |} | ||
<br clear="all"/> | |||
==Etching Si without back side cooling== | |||
{{Template:Author-bghe-thissection}} | |||
Etching in an ICP as the ASE without backside cooling normally results in heating up the sample to more than 100 degrees Celsius. This can be problematic especially when using resist as a masking material. <br> | |||
Etching in an ICP as the ASE without backside cooling normally results in heating up the sample to more than 100 degrees Celsius. This can be problematic especially | |||
There can be many reasons for not applying cooling to the sample. Among these are samples that need to be processed on a carrier due to sensitive backsides, sticky backsides or structures on the backside, small samples, membranes that can break, bowing wafers or something else. <br> | There can be many reasons for not applying cooling to the sample. Among these are samples that need to be processed on a carrier due to sensitive backsides, sticky backsides or structures on the backside, small samples, membranes that can break, bowing wafers or something else. <br> | ||
To meet these needs we have developed a silicon etch in the RIE mode where the coil power is not being used. The coil creates a high density plasma and that has a higher plasma temperature | To meet these needs we have developed a silicon etch in the RIE mode where the coil power is not being used. The coil creates a high density plasma and that has a higher plasma temperature than a low density plasma created by the platen power in RIE mode. <br> | ||
This recipe is intended to only for low etch depths that are not very critical with regards to eg. the sidewall profile. For deep etching of silicon you will need to use the bosch process and the coil power. | |||
''' Recipe name in the ASE: "1si_rie1" ''' | |||
{| border="1" cellspacing="1" cellpadding="1" align="left" | |||
! Wafer ID | |||
! '''Resist before etch''' | |||
! '''Platen power''' | |||
! '''Pressure''' | |||
! '''Flow rate SF6''' | |||
! '''Flow rate O2''' | |||
! '''Flow rate Ar''' | |||
! width="20"| '''T''' | |||
! '''Process time''' | |||
! '''Comment''' | |||
! width="205"|'''Results''' | |||
! '''CD change''' | |||
! '''Profile angles''' | |||
! width="150"|'''Etch rate in Si''' | |||
! '''Etch rate in resist''' | |||
! '''Selectivity (resist:Si)''' | |||
! '''Etch rate in SiO2''' | |||
|- | |||
|- | |||
|-style="background:white; color:black" | |||
|ASE RIE9 | |||
|<!-- '''Resist before etch''' --> 3750nm | |||
|<!--'''Platen power'''--> 100W | |||
|<!--'''Pressure'''--> 80mTorr | |||
|<!--'''Flow rate CF4'''--> 40sccm | |||
|<!--'''Flow rate O2'''--> 27sccm | |||
|<!--'''Flow rate Ar'''-->0 | |||
|<!--'''T'''--> 20 | |||
|<!--'''Process time'''--> 30min | |||
|<!--'''Comment'''--> HBC off, resist not burned. Microscope images! | |||
|<!--'''Results'''-->[[File:ASE RIE9 d.jpg|200px]][[File:ASE RIE9 f.jpg|200px]] | |||
|<!--'''CD change (mask 55% trench) after s007467 is it <50% after barc etch'''<br> | |||
trench opening as a fraction of pitch--> | |||
. | |||
|<!--'''Profile angles'''--> | |||
. | |||
|<!--'''Etch rate in Si'''--> | |||
443.3 nm/min | |||
|<!--'''Etch rate in resist'''--> | |||
91.7 nm/min | |||
|<!--'''Selectivity (resist:Si)'''--> | |||
1:4.8 | |||
|<!--'''Etch rate in SiO2'''--> | |||
32 nm/min | |||
SRN:60 nm/min | |||
|- | |||
|-style="background:white; color:black" | |||
|ASE RIE8 | |||
|<!-- '''Resist before etch''' --> 3750nm | |||
|<!--'''Platen power'''--> 100W | |||
|<!--'''Pressure'''--> 80mTorr | |||
|<!--'''Flow rate CF4'''--> 40sccm | |||
|<!--'''Flow rate O2'''--> 27sccm | |||
|<!--'''Flow rate Ar'''-->0 | |||
|<!--'''T'''--> 20 | |||
|<!--'''Process time'''--> 4min | |||
|<!--'''Comment'''--> HBC off Microscope images! | |||
|<!--'''Results'''-->[[File:ASE RIE8 b.jpg|200px]][[File:ASE RIE8 c.jpg|200px]] | |||
|<!--'''CD change (mask 55% trench) after s007467 is it <50% after barc etch'''<br> | |||
trench opening as a fraction of pitch--> | |||
. | |||
|<!--'''Profile angles'''--> | |||
. | |||
|<!--'''Etch rate in Si'''--> | |||
440 nm/min | |||
|<!--'''Etch rate in resist'''--> | |||
nm/min | |||
|<!--'''Selectivity (resist:Si)'''--> | |||
|<!--'''Etch rate in Si'''--> | |||
? | |||
|} | |||