Specific Process Knowledge/Etch/DRIE-Pegasus/nanoetch/nano13: Difference between revisions
Appearance
No edit summary |
|||
| (7 intermediate revisions by 2 users not shown) | |||
| Line 1: | Line 1: | ||
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/DRIE-Pegasus/nanoetch/nano13 click here]''' | |||
<!--Checked for updates on 30/7-2018 - ok/jmli --> | |||
<!--Checked for updates on 5/10-2020 - ok/jmli --> | |||
<!--Checked for updates on 4/9-2025 - ok/jmli --> | |||
== The nano1.3 recipe == | == The nano1.3 recipe == | ||
{{Template:Author-jmli1}} | |||
<!--Checked for updates on 2/02-2023 - ok/jmli --> | |||
{| border="2" cellpadding="2" cellspacing="1" | {| border="2" cellpadding="2" cellspacing="1" | ||
| Line 31: | Line 37: | ||
|- | |- | ||
| Mask | | Mask | ||
| | | 211 nm zep etched down 117 nm | ||
|- | |- | ||
|} | |} | ||
| Line 50: | Line 56: | ||
</gallery> | </gallery> | ||
{| {{table}} | |||
|+ After 60 seconds | |||
| align="center" style="background:#f0f0f0;"|'''Nominal trench line width''' | |||
| align="center" style="background:#f0f0f0;"|'''''' | |||
| align="center" style="background:#f0f0f0;"|'''30''' | |||
| align="center" style="background:#f0f0f0;"|'''60''' | |||
| align="center" style="background:#f0f0f0;"|'''90''' | |||
| align="center" style="background:#f0f0f0;"|'''120''' | |||
| align="center" style="background:#f0f0f0;"|'''150''' | |||
| align="center" style="background:#f0f0f0;"|'''Avg''' | |||
| align="center" style="background:#f0f0f0;"|'''Std''' | |||
|- | |||
| ER||nm/min||241||285||307||325||335||299||37 | |||
|- | |||
| SA||degs||92||92||92||91||91||92||0 | |||
|- | |||
| base||nm/edge||-5||-8||-18||-18||-34||-17||11 | |||
|- | |||
| foot||nm/edge||-5||-8||-18||-18||-4||-10||7 | |||
|- | |||
| Bowing||||19||11||11||14||10||13||4 | |||
|- | |||
| Curve||||-48||-46||-43||-40||-40||-44||4 | |||
|- | |||
| zep||nm/min||||||||||||95|| | |||
|- | |||
| | |||
|} | |||
{| {{table}} | |||
|+ After 120 seconds | |||
| align="center" style="background:#f0f0f0;"|'''Nominal trench line width''' | |||
| align="center" style="background:#f0f0f0;"|'''''' | |||
| align="center" style="background:#f0f0f0;"|'''30''' | |||
| align="center" style="background:#f0f0f0;"|'''60''' | |||
| align="center" style="background:#f0f0f0;"|'''90''' | |||
| align="center" style="background:#f0f0f0;"|'''120''' | |||
| align="center" style="background:#f0f0f0;"|'''150''' | |||
| align="center" style="background:#f0f0f0;"|'''Average''' | |||
| align="center" style="background:#f0f0f0;"|'''Std. dev.''' | |||
|- | |||
| ER||nm/min||189||195||229||241||242||219||25 | |||
|- | |||
| SA||degs||95||93||93||93||94||94||1 | |||
|- | |||
| base||nm/edge||0||4||-6||-26||-34||-13||17 | |||
|- | |||
| foot||nm/edge||5||16||6||-12||-7||2||12 | |||
|- | |||
| Bowing||||27||12||30||22||30||24||7 | |||
|- | |||
| Curve||||-56||-54||-45||-40||-45||-48||7 | |||
|- | |||
| zep||nm/min||||||||||||81|| | |||
|- | |||
| | |||
|} | |||
Latest revision as of 10:27, 4 September 2025
Feedback to this page: click here
The nano1.3 recipe
Unless otherwise stated, all content on this page was created by Jonas Michael-Lindhard, DTU Nanolab
| Recipe | Gas | C4F8 38 sccm, SF6 52 sccm |
|---|---|---|
| Pressure | 4 mTorr, Strike 3 secs @ 15 mTorr | |
| Power | 600 W CP, 40 W PP | |
| Temperature | -10 degs | |
| Hardware | 100 mm Spacers | |
| Time | 60 secs (a) and 120 secs (b) | |
| Conditions | Run ID | (a) 1856 and (b) 1856+1857 |
| Conditioning | Sequence: Oxygen clean, processes, no oxygen between runs | |
| Mask | 211 nm zep etched down 117 nm |
- The results of the nano1.3 recipe
-
The 30 nm trenches after 60 secs.
-
The 60 nm trenches after 60 secs.
-
The 90 nm trenches after 60 secs.
-
The 120 nm trenches after 60 secs.
-
The 150 nm trenches after 60 secs.
-
The 30 nm trenches after 120 secs.
-
The 60 nm trenches after 120 secs.
-
The 90 nm trenches after 120 secs.
-
The 120 nm trenches after 120 secs.
-
The 150 nm trenches after 120 secs.
| Nominal trench line width | ' | 30 | 60 | 90 | 120 | 150 | Avg | Std |
| ER | nm/min | 241 | 285 | 307 | 325 | 335 | 299 | 37 |
| SA | degs | 92 | 92 | 92 | 91 | 91 | 92 | 0 |
| base | nm/edge | -5 | -8 | -18 | -18 | -34 | -17 | 11 |
| foot | nm/edge | -5 | -8 | -18 | -18 | -4 | -10 | 7 |
| Bowing | 19 | 11 | 11 | 14 | 10 | 13 | 4 | |
| Curve | -48 | -46 | -43 | -40 | -40 | -44 | 4 | |
| zep | nm/min | 95 | ||||||
| Nominal trench line width | ' | 30 | 60 | 90 | 120 | 150 | Average | Std. dev. |
| ER | nm/min | 189 | 195 | 229 | 241 | 242 | 219 | 25 |
| SA | degs | 95 | 93 | 93 | 93 | 94 | 94 | 1 |
| base | nm/edge | 0 | 4 | -6 | -26 | -34 | -13 | 17 |
| foot | nm/edge | 5 | 16 | 6 | -12 | -7 | 2 | 12 |
| Bowing | 27 | 12 | 30 | 22 | 30 | 24 | 7 | |
| Curve | -56 | -54 | -45 | -40 | -45 | -48 | 7 | |
| zep | nm/min | 81 | ||||||