== The nano1.4 recipe == | == The nano1.4 recipe == | ||
{{Template:Author-jmli1}} | |||
<!--Checked for updates on 2/02-2023 - ok/jmli --> | |||
{| border="2" cellpadding="2" cellspacing="1" | {| border="2" cellpadding="2" cellspacing="1" | ||
| Line 31: | Line 39: | ||
|- | |- | ||
| Mask | | Mask | ||
| | | 211 nm zep etched down to 77 nm | ||
|- | |- | ||
|} | |} | ||
| Line 44: | Line 52: | ||
C4F8 75 sccm, SF6 38 sccm, 4 mTorr, Strike 3 secs @ 15 mTorr, 800 W CP, 50 W PP, -20 degs, 120 secs | C4F8 75 sccm, SF6 38 sccm, 4 mTorr, Strike 3 secs @ 15 mTorr, 800 W CP, 50 W PP, -20 degs, 120 secs | ||
</gallery> | </gallery> | ||
{| {{table}} | |||
| align="center" style="background:#f0f0f0;"|'''Nominal trench line width''' | |||
| align="center" style="background:#f0f0f0;"|'''''' | |||
| align="center" style="background:#f0f0f0;"|'''30''' | |||
| align="center" style="background:#f0f0f0;"|'''60''' | |||
| align="center" style="background:#f0f0f0;"|'''90''' | |||
| align="center" style="background:#f0f0f0;"|'''120''' | |||
| align="center" style="background:#f0f0f0;"|'''150''' | |||
| align="center" style="background:#f0f0f0;"|'''Average''' | |||
| align="center" style="background:#f0f0f0;"|'''Std. dev.''' | |||
|- | |||
| Etch rates||nm/min||168||182||185||189||191||183||9 | |||
|- | |||
| Sidewall angle||degs||91||91||91||91||90||91||0 | |||
|- | |||
| CD loss||nm/edge||7||-3||-3||-25||-26||-10||15 | |||
|- | |||
| CD loss foot||nm/edge||12||9||10||-11||1||4||9 | |||
|- | |||
| Bowing||||9||6||4||5||7||6||2 | |||
|- | |||
| Bottom curvature||||-47||-34||-34||-26||-19||-32||10 | |||
|- | |||
| zep||nm/min||||||||||||67|| | |||
|- | |||
| | |||
|} | |||