Jump to content

Specific Process Knowledge/Etch/ICP Metal Etcher/Titanium: Difference between revisions

From LabAdviser
Jmli (talk | contribs)
No edit summary
Jmli (talk | contribs)
No edit summary
 
(2 intermediate revisions by the same user not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Etch/ICP_Metal_Etcher/Titanium click here]'''  
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/ICP_Metal_Etcher/Titanium click here]'''  
 
<!--Checked for updates on 5/10-2020 - ok/jmli -->
<!--Checked for updates on 30/7-2018 - ok/jmli -->
<!--Checked for updates on 30/7-2018 - ok/jmli -->
<!--Checked for updates on 4/9-2025 - ok/jmli -->


=== Titanium etch ===
=== Titanium etch ===
{{Template:Author-jmli1}}
<!--Checked for updates on 2/02-2023 - ok/jmli -->





Latest revision as of 10:25, 4 September 2025

Feedback to this page: click here

Titanium etch

Unless otherwise stated, all content on this page was created by Jonas Michael-Lindhard, DTU Nanolab


Ti etch
Parameter Process 1 Process 2
Cl2 (sccm) 30 30
HBr (sccm) - -
Pressure (mTorr) 3, Strike 3 secs @ 15 mTorr??? 3
Coil power (W) 800 900
Platen power (W) 100 50
Temperature (oC) 20 20
Spacers (mm) 30 30
Etch rate (nm/min) 152 64
AZ resist selectivity 0.67 0.83