Specific Process Knowledge/Etch/DRIE-Pegasus/nanoetch: Difference between revisions
Appearance
No edit summary |
No edit summary |
||
| (One intermediate revision by the same user not shown) | |||
| Line 2: | Line 2: | ||
<!--Checked for updates on 30/7-2018 - ok/jmli --> | <!--Checked for updates on 30/7-2018 - ok/jmli --> | ||
<!--Checked for updates on 5/10-2020 - ok/jmli --> | <!--Checked for updates on 5/10-2020 - ok/jmli --> | ||
<!--Checked for updates on 4/9-2025 - ok/jmli --> | |||
== Development of continuous nanoetch == | == Development of continuous nanoetch == | ||
{{Template:Author-jmli1}} | |||
<!--Checked for updates on 2/02-2023 - ok/jmli --> | |||
The recipes below have been run on 2" wafers with 30/60/90/120/150 nm lines in zep resist. The wafers were crystalbonded to a 4" oxide carrier leaving only a very small fraction (much less than 1% ) of silicon to be etched. If you intend to etch most of the surface of the wafer to create very small posts or ridges (rather than holes or trenches) | The recipes below have been run on 2" wafers with 30/60/90/120/150 nm lines in zep resist. The wafers were crystalbonded to a 4" oxide carrier leaving only a very small fraction (much less than 1% ) of silicon to be etched. If you intend to etch most of the surface of the wafer to create very small posts or ridges (rather than holes or trenches) | ||
Latest revision as of 10:25, 4 September 2025
Feedback to this page: click here
Development of continuous nanoetch
Unless otherwise stated, all content on this page was created by Jonas Michael-Lindhard, DTU Nanolab
The recipes below have been run on 2" wafers with 30/60/90/120/150 nm lines in zep resist. The wafers were crystalbonded to a 4" oxide carrier leaving only a very small fraction (much less than 1% ) of silicon to be etched. If you intend to etch most of the surface of the wafer to create very small posts or ridges (rather than holes or trenches)
The most used one is the nano1.42 recipe - to access the results, click on the bold link in the bottom of the table.
| Recipe | nano1.0 | nano1.1 | nano1.2 | nano1.3 | nano1.21 | nano1.4 | nano1.41 | nano1.42 | nano1.43 |
|---|---|---|---|---|---|---|---|---|---|
| C4F8 (sccm) | 52 | 52 | 52 | 52 | 75 | 75 | 75 | 75 | 75 |
| SF6 (sccm) | 38 | 38 | 38 | 38 | 38 | 38 | 38 | 38 | 38 |
| O2 (sccm) | 0 | 0 | 0 | 0 | 0 | 0 | 0 | 0 | 0 |
| Coil power (W) | 800 (F) | 600 (F) | 800 (F) | 600 (F) | 800 (F) | 800 (F) | 800 (F) | 800 (F) | 800 (F) |
| Platen power (W) | 50 | 50 | 50 | 40 | 50 | 50 | 75 | 40 | 30 |
| Pressure (mtorr) | 4 | 4 | 4 | 4 | 4 | 4 | 4 | 4 | 4 |
| Temperature (degs C) | 10 | 10 | -10 | -10 | -10 | -20 | -20 | -20 | -20 |
| Process time (s) | 120 | 120 | 120 | 120 | 120 | 120 | 120 | 120 | 120 |
| Etch rates (nm/min) | |||||||||
| Averages | 295 | 228 | 299 | 235 | 183 | 183 | 166 | 160 | 148 |
| Std. Dev | 36 | 29 | 37 | 20 | 9 | 9 | 9 | 8 | 6 |
| Zep etch rate (nm/min) | |||||||||
| 172 | 95 | 94 | 69 | 67 | 101 | 65 | 55 | ||
| Sidewall angle (degrees) | |||||||||
| Averages | 93 | 94 | 92 | 94 | 91 | 91 | 90 | 90 | 90 |
| Std. Dev | 1 | 1 | 0 | 1 | 0 | 0 | 1 | 0 | 0 |
| CD loss (nm pr edge) | |||||||||
| Averages | -11 | -13 | -17 | -10 | -10 | -10 | -20 | -13 | -24 |
| Std. Dev | 12 | 10 | 11 | 14 | 15 | 15 | 16 | 15 | 21 |
| Bowing (nm) | |||||||||
| Averages | 31 | 42 | 13 | 16 | 6 | 6 | 3 | -3 | 0 |
| Std. Dev | 7 | 6 | 4 | 3 | 2 | 2 | 2 | 3 | 1 |
| Bottom curvature | |||||||||
| Averages | -45 | -45 | -44 | -43 | -32 | -32 | -34 | -32 | -39 |
| Std. Dev | 5 | 7 | 4 | 9 | 10 | 10 | 9 | 8 | 9 |
| Images | Images | Images | Images | Images | Images | Images | Images | Images | Images |
- Etch of nanostructures in silicon on the ICP Metal Etcher
- Nanoetch contest: DRIE-Pegasus versus ASE (nano1.42 versus pxnano2)
Development of switched nanoetch process
On the basis of the pxnano2 recipe from the ASE we will try to make a similar Bosch process on the Pegasus.
| Recipe | Step | Temp. | Deposition step | Etch step | Process observations | ||||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Time | Pressure | C4F8 | SF6 | O2 | Coil | Time | Pressure | C4F8 | SF6 | O2 | Coil | Platen | Hardware | Runs | |||
| nanobosch6 | A | 20 | 2.5 | 10 | 50 | 0 | 0 | 500 | 5.0 | 10 | 40 | 60 | 5 | 350 | 30 | LF+B100 | Click |
| nb-1.0 | A | 20 | 2.5 | 10 | 50 | 0 | 0 | 500 | 5.0 | 10 | 50 | 50 | 5 | 350 | 30 | LF+B100 | Click |
| nb-1.1 | A | 20 | 2.5 | 10 | 50 | 0 | 0 | 500 | 5.0 | 10 | 50 | 50 | 5 | 350 | 50 | LF+B100 | Click |
| nb-1.2 | A | 20 | 2.5 | 10 | 50 | 0 | 0 | 500 | 5.0 | 10 | 50 | 50 | 5 | 500 | 50 | LF+B100 | Click |
| barcstrip | A | 20 | 30 | 4 (3@15) | 0 | 0 | 40 | 200 | 20 | LF+B100 | Click | ||||||
| nanobosch7 | A | 20 | 2.5 | 10 | 50 | 0 | 0 | 500 | 5.0 | 10 | 40 | 60 | 5 | 350 | 30 | LF+B100 | Click |
| LF+B100 | Click | ||||||||||||||||